MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Hexcel® Hexcel Tooling Fabrics
Categories: Polymer; Thermoset; Bismaleimide (BMI); Carbon Fiber/Thermoset Composite

Material Notes: Hexcel tooling fabrics are produced from high-performance bismaleimide (BMI) resin and carbon fiber utilizing Hexcel’s proprietary PrimeTex® spreading technology. PrimeTex® fabrics are inherently more uniform as the filaments in each tow are spread creating a closed fabric with lower interstitial porosity and reduced resin rich regions normally seen in other tooling fabrics. The resulting tooling surface enables quality part production with less post cure processing of finished part surfaces. The unique combination of Hexcel’s advanced tooling fabrics and Hexcel’s high Tg M61 resin system create a product capable of high production rate-durable low mass carbon tools.

Benefits

  • PrimeTex® fabrics have reduced resin-rich pockets resulting in higher durability and enhanced part quality
  • High Tg resulting in high-rate tools for 350°F cure.
  • Available in either standard modulus or intermediate modulus 3, 6 and 12K fibers
  • High fiber volume fraction
  • Excellent tack and drape
  • Excellent out-time

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Viscosity >= 2240 cP>= 2240 cP
 
Mechanical PropertiesMetricEnglishComments
Hardness, Barcol 79.079.0Dry; ASTM D2583
Flexural Strength  575.8 MPa
@Temperature 191 °C
83510 psi
@Temperature 375 °F
0°; ASTM D 790
 625.5 MPa
@Temperature 191 °C
90720 psi
@Temperature 375 °F
0°, TA FL1; ASTM D 790
 762.28 MPa
@Temperature 21.1 °C
110560 psi
@Temperature 70.0 °F
0°, TA FL1; ASTM D 790
 821.72 MPa
@Temperature 21.1 °C
119180 psi
@Temperature 70.0 °F
0°; ASTM D 790
Flexural Modulus  0.0310 GPa
@Temperature 191 °C
4.50 ksi
@Temperature 375 °F
0°, TA FL1; ASTM D 790
 0.312 GPa
@Temperature 191 °C
45.2 ksi
@Temperature 375 °F
0°; ASTM D 790
 0.329 GPa
@Temperature 21.1 °C
47.7 ksi
@Temperature 70.0 °F
0°; ASTM D 790
 0.334 GPa
@Temperature 21.1 °C
48.4 ksi
@Temperature 70.0 °F
0°, TA FL1; ASTM D 790
Compressive Strength  224.4 MPa
@Temperature 191 °C
32550 psi
@Temperature 375 °F
Open Hole; ASTM D6484
 257.7 MPa
@Temperature 191 °C
37380 psi
@Temperature 375 °F
After Impact, TA FL1; ASTM D7316/D7317
 259 MPa
@Temperature 21.1 °C
37500 psi
@Temperature 70.0 °F
After Impact; ASTM D7316/D7317
 264.7 MPa
@Temperature 191 °C
38390 psi
@Temperature 375 °F
Open Hole, TA FL1; ASTM D6484
 316.1 MPa
@Temperature 21.1 °C
45850 psi
@Temperature 70.0 °F
Open Hole; ASTM D6484
 326.6 MPa
@Temperature 21.1 °C
47370 psi
@Temperature 70.0 °F
Open Hole, TA FL1; ASTM D6484
Shear Strength 80.94 MPa11740 psi0° Short Beam, 60 Day Out Time; ASTM D2344
 83.98 MPa
@Temperature 21.1 °C
12180 psi
@Temperature 70.0 °F
0° Short Beam; ASTM D2344
 
Thermal PropertiesMetricEnglishComments
CTE, linear 167 µm/m-°C92.8 µin/in-°F
 2.48 µm/m-°C
@Temperature 21.1 - 200 °C
1.38 µin/in-°F
@Temperature 70.0 - 392 °F
x direction
 2.489 µm/m-°C
@Temperature 21.1 - 200 °C
1.383 µin/in-°F
@Temperature 70.0 - 392 °F
y direction
 45.391 µm/m-°C
@Temperature 21.1 - 200 °C
25.217 µin/in-°F
@Temperature 70.0 - 392 °F
z direction
Maximum Service Temperature, Air 218 °C424 °FPost-cured
Glass Transition Temp, Tg 163 °C325 °FWet
 177 °C351 °FWet, Enhanced Post Cure
 218 °C424 °FDry
 232 °C450 °FDry, Enhanced Post Cure
 275 °C527 °F
Shrinkage -0.00100 %-0.00100 %After TA (30 inch long specimen) FL2
 
Processing PropertiesMetricEnglishComments
Cure Time 28800 min480 hourTack life
Shelf Life 12.0 Month
@Temperature -17.8 °C
12.0 Month
@Temperature -0.0400 °F
 
Descriptive Properties
Content0.38
Fabric Weight196 g/m23K; Plain Weave
 380 g/m26K; 8 Harness Satin
 670 g/m212K; 5 Harness Satin

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHEXCB9260 / 322416

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.