MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 2040 Epoxy Prepreg Unidirectional Tape with M55J-140
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: CYCOM® 2040 is a very tough modified epoxy resin system with exceptional high temperature performance. It is suitable for highly stressed components exposed to elevated temperature environments (under bonnet/engine bay) including impact/crash structures. A two hour cure at 180°C (356°F) generates a Tg of over 200°C (392°F)* and offers excellent mechanical properties at both ambient and elevated temperatures. CYCOM 2040 is available on woven and unidirectional carbon, glass and man-made fibers.

Features & Benefits:

  • High levels of mechanical property retention at elevated temperatures
  • Controlled flow
  • Excellent cured surface quality
  • Low cured resin density (1.21g/cm³)
  • Free-standing post curable to 200°C (356°F) for maximum temperature performance
  • Shop life of 21 days at ambient [23°C (73°F)]
  • Available in a wide range of fibers and fabric weaves
Suggested Applications:
  • Primary vehicle structures including chassis, engine frames suspension components and aerodynamic wings
  • Impact structures including nose cone, side and rear
  • Components requiring operating temperatures up to 200°C (392°F)
Nominal reinforcement content for reported properties is 36% M55J-140.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.21 g/ccCured Unfilled Resin
Viscosity >= 16000 cP
@Temperature 150 °C
Neat Resin
Storage Temperature <= -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 3900 psi
@Temperature 150 °C
90° orientation, Actual 52.4% VF
 5100 psi
@Temperature 24.0 °C
90° orientation, Actual 52.4% VF
 210000 psi
@Temperature 150 °C
0° orientation, Actual 54.2% VF
 235000 psi
@Temperature 24.0 °C
0° orientation, Actual 54.2% VF
 240000 psi
@Temperature 150 °C
0° orientation, Normalized 60% VF
 269000 psi
@Temperature 24.0 °C
0° orientation, Normalized 60% VF
Tensile Modulus 4.74 GPa
@Temperature 150 °C
90° orientation, Actual 52.4% VF
 5.62 GPa
@Temperature 24.0 °C
90° orientation, Actual 52.4% VF
 283 GPa
@Temperature 150 °C
0° orientation, Actual 54.2% VF
 297 GPa
@Temperature 24.0 °C
0° orientation, Actual 54.2% VF
 323 GPa
@Temperature 150 °C
0° orientation, Normalized 60% VF
 339 GPa
@Temperature 24.0 °C
0° orientation, Normalized 60% VF
Flexural Strength 127000 psi
@Temperature 150 °C
0° orientation, Actual 54.2% VF
 140000 psi
@Temperature 24.0 °C
0° orientation, Actual 54.2% VF
 144000 psi
@Temperature 150 °C
0° orientation, Normalized 60% VF
 160000 psi
@Temperature 24.0 °C
0° orientation, Normalized 60% VF
Flexural Modulus 233 GPa
@Temperature 24.0 °C
0° orientation, Actual 54.2% VF
 251 GPa
@Temperature 150 °C
0° orientation, Actual 54.2% VF
 265 GPa
@Temperature 24.0 °C
0° orientation, Normalized 60% VF
 285 GPa
@Temperature 150 °C
0° orientation, Normalized 60% VF
Compressive Strength 93.9 MPa
@Temperature 150 °C
90° orientation, Actual 52.4% VF
 190.6 MPa
@Temperature 24.0 °C
90° orientation, Actual 52.4% VF
 495 MPa
@Temperature 150 °C
0° orientation, Actual 54.2% VF
 573 MPa
@Temperature 150 °C
0° orientation, Normalized 60% VF
 600 MPa
@Temperature 24.0 °C
0° orientation, Actual 54.2% VF
 695 MPa
@Temperature 24.0 °C
0° orientation, Normalized 60% VF
Compressive Modulus 5750 MPa
@Temperature 150 °C
90° orientation, Actual 52.4% VF
 6080 MPa
@Temperature 24.0 °C
90° orientation, Actual 52.4% VF
 246000 MPa
@Temperature 150 °C
0° orientation, Actual 54.2% VF
 263000 MPa
@Temperature 24.0 °C
0° orientation, Actual 54.2% VF
 285000 MPa
@Temperature 150 °C
0° orientation, Normalized 60% VF
 305000 MPa
@Temperature 24.0 °C
0° orientation, Normalized 60% VF
Poissons Ratio 0.90
@Temperature 24.0 °C
±45°, Actual 52.4% VF
 0.96
@Temperature 150 °C
±45°, Actual 52.4% VF
Shear Modulus 2.72 GPa
@Temperature 150 °C
In Plane, Actual 52.4% VF
 4.60 GPa
@Temperature 24.0 °C
In Plane, Actual 52.4% VF
Shear Strength 6900 psi
@Temperature 150 °C
Interlaminar, Actual 52.4% VF
 7700 psi
@Temperature 150 °C
In Plane, Actual 52.4% VF
 8200 psi
@Temperature 24.0 °C
In Plane, Actual 52.4% VF
 9800 psi
@Temperature 24.0 °C
Interlaminar, Actual 52.4% VF
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 200 °C
Glass Transition Temp, Tg >= 200 °Cfollowing 180°C (356°F) cure
 
Processing PropertiesOriginal ValueComments
Gel Time 58.0 min
@Temperature 167 °C
Shelf Life 12.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 950-1 Epoxy Prepreg Unidirectional Tape with 36%-M55J-140 GSM
Solvay CYCOM® 2040 Epoxy Prepreg Fabric with 6KM46J-2X2T-200
Solvay CYCOM® 977-6 Epoxy Prepreg Laminate with M55J-140-300 Unidirectional Tape
Solvay CYCOM® 5250-4 BMI Prepreg System with IM-7 Carbon Fiber
Solvay CYCOM® 2020 Epoxy + M46J 140 Unidirectional Tape Prepreg, without Post-Cure

PCYTED132_1 / 192674

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.