MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
BCC Products BC 8990 Polyurethane Elastomer
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced; Rubber or Thermoset Elastomer (TSE)

Material Notes: BC8990 is a two-component urethane elastomer compound specifically designed for general purpose molding and casting of various shapes. This product is a safe, easy-to-handle, room temperature mixing and curing system that contains no TDI, MDA or MOCA. BC8990 may be used to provide abrasion resistant liners, pads and bumpers. The low shrinkage, low viscosity, superior toughness, and excellent detail reproduction of makes this system ideal for general purpose castings and quality tooling operations. It may also be used in potting and encapsulating applications.

Information provided by BCC Products, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.03 g/ccASTM D792
Brookfield Viscosity 50 cP
@Temperature 23.9 °C
Part B; ASTM D2393
 3600 cP
@Temperature 23.9 °C
initial mixed; ASTM D2393
 6000 cP
@Temperature 23.9 °C
Part A; ASTM D2393
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 82 - 85ASTM D2240
Tensile Strength, Ultimate 1750 psiASTM D412
Elongation at Break 720 %ASTM D412
Tensile Modulus 550 psi100%; ASTM D412
Tear Strength 175 pliASTM 4-624-54 Die C
 
Processing PropertiesOriginal ValueComments
Cure Time 960 - 1440 min
@Temperature 24.0 °C
demold time
 4320 - 7200 min
@Temperature 24.0 °C
full cure
Gel Time 25 min
@Temperature 24.0 °C
ASTM D2471
 
Descriptive Properties
Mix Ratio4:1 by weight (A/B)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BCC Products BC 8860 Polyurethane Elastomer
BCC Products BC 8690E Polyurethane Elastomer
BCC Products BC 8675E Polyurethane Elastomer
BCC Products BC 8870 Polyurethane Elastomer
Fibre Glast 1110 CC Vinyl Ester Resin (Casting Properties)

PBCC070 / 107297

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.