MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Arkema Kynar® 720 MED PVDF
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF); Polyvinylidinefluoride (PVDF), Molded/Extruded

Material Notes:

Information provided by Arkema Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.77 - 1.79 g/cc1.77 - 1.79 g/ccASTM D792
Density 1.78 g/cc0.0643 lb/in³ISO 1183
Water Absorption 0.010 - 0.030 %0.010 - 0.030 %ASTM D570
 0.020 %0.020 %Dry; Sim. to ISO 62
Moisture Absorption 0.0150 %0.0150 %Dry; Sim. to ISO 62
Viscosity 600000 - 1.20e+6 cP
@Shear Rate 100 1/s,
Temperature 230 °C
600000 - 1.20e+6 cP
@Shear Rate 100 1/s,
Temperature 446 °F
Melt; ASTM D3835
Linear Mold Shrinkage, Flow 0.020 cm/cm0.020 in/inDry; ISO 294-4, 2577
 0.020 cm/cm0.020 in/in
Melt Flow  14.8 g/10 min
@Load 3.80 kg,
Temperature 230 °C
14.8 g/10 min
@Load 8.38 lb,
Temperature 446 °F
cm³/10 min Volumetric Rate; ISO 1133
 14 - 26.5 g/10 min
@Load 3.80 kg,
Temperature 230 °C
14 - 26.5 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 76 - 8076 - 80ASTM D2240
Tensile Strength at Break 34.5 - 55.2 MPa5000 - 8010 psiASTM D638
Tensile Strength, Yield 44.8 - 55.2 MPa6500 - 8010 psiASTM D638
 54.0 MPa7830 psiDry; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Dry; ISO 527-1/-2
 20 - 100 %20 - 100 %ASTM D638
Elongation at Yield 5.0 - 10 %5.0 - 10 %ASTM D638
 8.0 %8.0 %Dry; ISO 527-1/-2
Tensile Modulus 1.38 - 2.31 GPa200 - 335 ksiASTM D638
 2.20 GPa319 ksiDry; ISO 527-1/-2
Flexural Strength 58.6 - 75.8 MPa
@Strain 5.0 %
8500 - 11000 psi
@Strain 5.0 %
ASTM D790
Flexural Modulus 1.38 - 2.31 GPa200 - 335 ksiASTM D790
Compressive Strength 68.9 - 103 MPa9990 - 14900 psiASTM D695
Izod Impact, Notched 0.801 - 2.14 J/cm1.50 - 4.01 ft-lb/inASTM D256
Izod Impact, Unnotched 10.7 - 42.7 J/cm20.0 - 80.0 ft-lb/inASTM D256
Charpy Impact Unnotched  18.9 J/cm²
@Temperature -30.0 °C
89.9 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 20.8 J/cm²
@Temperature 23.0 °C
99.0 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  0.500 J/cm²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.800 J/cm²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
Coefficient of Friction, Dynamic 0.140.14vs. steel; ASTM D1894
Coefficient of Friction, Static 0.200.20vs. steel; ASTM D1894
Taber Abrasion, mg/1000 Cycles 5.0 - 9.05.0 - 9.0CS 17 1000g:pad; ASTM-G195-13A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2.00e+14 ohm-cm2.00e+14 ohm-cmDry; IEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmCond.; IEC 60093
Dielectric Constant  4.5 - 9.5
@Frequency 1000 Hz
4.5 - 9.5
@Frequency 1000 Hz
ASTM D150
 7.0
@Frequency 1e+6 Hz
7.0
@Frequency 1e+6 Hz
Dry; IEC 60250
 9.0
@Frequency 100 Hz
9.0
@Frequency 100 Hz
Dry; IEC 60250
Dielectric Strength 21.0 kV/mm533 kV/inDry; IEC 60243-1
Dissipation Factor  0.032
@Frequency 100 Hz
0.032
@Frequency 100 Hz
Dry; IEC 60250
 0.010 - 0.21
@Frequency 100000 Hz
0.010 - 0.21
@Frequency 100000 Hz
ASTM D150
 0.214
@Frequency 1e+6 Hz
0.214
@Frequency 1e+6 Hz
Dry; IEC 60250
Comparative Tracking Index 600 V600 VDry; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 214 - 259 µm/m-°C119 - 144 µin/in-°FASTM D696
CTE, linear, Parallel to Flow 130 µm/m-°C72.2 µin/in-°FDry; ISO 11359-1/-2
Specific Heat Capacity 0.745 - 0.958 J/g-°C0.178 - 0.229 BTU/lb-°FDSC
Thermal Conductivity 0.170 - 0.190 W/m-K1.18 - 1.32 BTU-in/hr-ft²-°FASTM D433
Melting Point 168 °C334 °F10°C/min; Dry; ISO 11357-1/-3
 165 - 172 °C329 - 342 °FASTM D3418
Maximum Service Temperature, Air 150 °C302 °FUL RTI
Deflection Temperature at 0.46 MPa (66 psi) 132 °C270 °FDry; ISO 75-1/-2
 125 - 140 °C257 - 284 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 108 °C226 °FDry; ISO 75-1/-2
 105 - 115 °C221 - 239 °FASTM D648
Vicat Softening Point 139 °C282 °F50°C/h 50N; Dry; ISO 306
Glass Transition Temp, Tg -40.0 °C-40.0 °F10°C/min; Dry; ISO 11357-1/-2
 -40.6 - -38.3 °C-41.1 - -36.9 °FASTM D7028
Decomposition Temperature 375 °C707 °F1% wt. loss, TGA, in air
 410 °C770 °F1% wt. loss, TGA, in nitrogen
UL RTI, Electrical 150 °C302 °FUL 746B
UL RTI, Mechanical without Impact 150 °C302 °FUL 746B
Flammability, UL94  V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
IEC 60695-11-10
 V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
Yellow Card Available; Dry; IEC 60695-11-10
Oxygen Index 43 %43 %Dry; ISO 4589-1/-2
 >= 44 %>= 44 %
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.421.42sodium D line; ASTM D542
 
Processing PropertiesMetricEnglishComments
Melt Temperature 190 - 270 °C374 - 518 °F
 230 °C446 °FInjection Molding; ISO 294
Mold Temperature 23.0 - 90.0 °C73.4 - 194 °F
 90.0 °C194 °FInjection Molding; ISO 10724
 
Descriptive Properties
Form as DeliveredPellets
Moisture SensitiveNo

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PARKG905a / 291170

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.