MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 242.0-T21, Sand Cast
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes:

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 242.0-T21; UNS A02420; ISO 3522 and R164 AlCu4Ni2Mg2; AA242.0-T21; Al242.0-T21
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.823 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 70500 kg load, 10 mm ball
Hardness, Knoop 93Estimated from Brinell Hardness.
Hardness, Vickers 80Estimated from Brinell Hardness.
Tensile Strength, Ultimate 185 MPa
Tensile Strength, Yield 125 MPa
@Strain 0.2 %
Elongation at Break 2.0 %in 50 mm
Tensile Modulus 71.0 GPaCompressive modulus in is typically about 2% higher for Al alloys
Compressive Yield Strength 125 MPa
Poissons Ratio 0.33
Fatigue Strength 55.0 MPa
@# of Cycles 5.00e+8
Notch Status unknown, R.R. Moore Test
Machinability 70 %0-100 Scale (100=best)
Shear Modulus 26.5 GPa
Shear Strength 145 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000392 ohm-cm
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 389 J/g
CTE, linear 22.7 µm/m-°C
@Temperature 20.0 - 100 °C
 24.5 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.963 J/g-°C
Thermal Conductivity 167 W/m-K
Melting Point 532 - 635 °C
Solidus 532 °C
Liquidus 635 °C
 
Processing PropertiesOriginal ValueComments
Melt Temperature 1250 - 1500 °F
Annealing Temperature 645 - 655 °F2 - 4 hrs
Solution Temperature 965 - 975 °F
Casting Temperature 1250 - 1450 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 88.3 - 93.6 %As remainder
Chromium, Cr <= 0.25 %
Copper, Cu 3.5 - 4.5 %
Iron, Fe <= 1.0 %
Magnesium, Mg 1.2 - 1.8 %
Manganese, Mn <= 0.35 %
Nickel, Ni 1.7 - 2.3 %
Other, each <= 0.050 %
Other, total <= 0.15 %
Silicon, Si <= 0.70 %
Titanium, Ti <= 0.25 %
Zinc, Zn <= 0.35 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 242.0-O, Sand Cast
Aluminum 242.0-T571, Permanent Mold Cast
Aluminum 242.0-T61, Sand Cast
Aluminum 242.0-T571, Sand Cast
Aluminum 242.0-T77, Sand Cast

MAC2420T21 / 9808

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.