MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Piezo Kinetics PKI 552 Lead Zirconate Titanate Piezoelectric
Categories: Ceramic; Oxide; Titanium Oxide; Zirconium Oxide; Piezoelectric

Material Notes: Denoted as Navy Type VI, this ceramic is used as sensors that require extremely high dielectric constant and large displacements. PKI 556 material has been slightly modified to give a higher g33 value, higher k33 , and lower loss factor. This formulation aids the design engineer by giving more flexibility within the type VI class of materials.

Elastic Compliance s11E (x 10-12 m²/n): 15.9.
Elastic Compliance s33E (x 10-12 m²/n): 20.2.

Property data at 25°C. Information supplied by Piezo Kinetics, Inc.

Key Words: PKI 552, PZT, Lead Zirconium Titanate; PbZrO3 - PbTiO3 Solid Solution; Oxides
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.60 g/cc
 
Mechanical PropertiesOriginal ValueComments
Modulus of Elasticity 60.0 GPa
Poissons Ratio 0.31
Shear Modulus 23.0 GPacalculated
 
Electrical PropertiesOriginal ValueComments
Curie Temperature 200 °C
Dielectric Constant 3400
@Frequency 1000 Hz
Dissipation Factor 0.022
@Frequency 1000 Hz
Piezoelectric Longitudinal Coupling Factor, k33 0.71
Piezoelectric Transverse Voltage Coefficient, d31, 10^-12 m/V -270
Piezoelectric Shear Charge Coefficient, d15, 10^-12 m/V 720
Piezoelectric Longitudinal Voltage Coefficient, g33, 10^-3 V-m/N 18.3
Piezoelectric Planar Coupling Factor, kp 0.63
Piezoelectric Mechanical Q 75
Piezoelectric Shear Coupling Factor, k15 0.67
Piezoelectric Longitudinal Charge Coefficient, d33, 10^-12 m/V 550
Piezoelectric Transverse Voltage Coefficient, g31, 10^-3 V-m/N -9.00
Piezoelectric Shear Voltage Coefficient, g15, 10^-3 V-m/N 23.9
Piezoelectric Transverse Coupling Factor, k31 0.36
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 120 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Piezo Kinetics PKI 532 Lead Zirconate Titanate Piezoelectric
Piezo Kinetics PKI 502 Navy Type II Lead Zirconate Titanate Piezoelectric
Piezo Kinetics PKI 556 Lead Zirconate Titanate Piezoelectric
Piezo Kinetics PKI 804 Navy Type III Lead Zirconate Titanate Piezoelectric
Piezo Kinetics 402 Lead Zirconate Titanate Piezoelectric

CPKI25 / 1710

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.