Physical Properties | Metric | English | Comments |
---|
Density | 1.11 g/cc | 0.0401 lb/in³ |
Water Absorption | 1.3 % @Time 86400 sec | 1.3 % @Time 24.0 hour |
Moisture Absorption at Equilibrium | 2.3 % | 2.3 % |
Linear Mold Shrinkage, Flow | 0.018 cm/cm @Thickness 2.00 mm | 0.018 in/in @Thickness 0.0787 in |
Linear Mold Shrinkage, Transverse | 0.016 cm/cm @Thickness 2.00 mm | 0.016 in/in @Thickness 0.0787 in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 42.0 MPa | 6090 psi |
| 46.0 MPa | 6670 psi |
Tensile Strength, Yield | 50.0 MPa | 7250 psi |
| 70.0 MPa | 10200 psi |
Elongation at Break | 17 % | 17 % |
| 40 % | 40 % |
Tensile Modulus | 2.125 GPa | 308.2 ksi |
| 3.04 GPa | 441 ksi |
Flexural Strength | 27.0 MPa | 3920 psi |
| 81.0 MPa | 11700 psi |
Flexural Modulus | 0.890 GPa | 129 ksi |
| 2.60 GPa | 377 ksi |
Izod Impact, Notched (ISO) | 8.00 kJ/m² @Temperature -40.0 °C | 3.81 ft-lb/in² @Temperature -40.0 °F |
| 9.00 kJ/m² @Temperature -30.0 °C | 4.28 ft-lb/in² @Temperature -22.0 °F |
| 10.0 kJ/m² @Temperature -40.0 °C | 4.76 ft-lb/in² @Temperature -40.0 °F |
| 10.0 kJ/m² @Temperature 23.0 °C | 4.76 ft-lb/in² @Temperature 73.4 °F |
| 15.0 kJ/m² @Temperature -30.0 °C | 7.14 ft-lb/in² @Temperature -22.0 °F |
| 37.0 kJ/m² @Temperature 23.0 °C | 17.6 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact Unnotched | NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
| NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
| NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
Charpy Impact, Notched | 0.600 J/cm² @Temperature -40.0 °C | 2.86 ft-lb/in² @Temperature -40.0 °F |
| 0.800 J/cm² @Temperature -40.0 °C | 3.81 ft-lb/in² @Temperature -40.0 °F |
| 1.00 J/cm² @Temperature -30.0 °C | 4.76 ft-lb/in² @Temperature -22.0 °F |
| 1.10 J/cm² @Temperature -30.0 °C | 5.23 ft-lb/in² @Temperature -22.0 °F |
| 1.30 J/cm² @Temperature 23.0 °C | 6.19 ft-lb/in² @Temperature 73.4 °F |
| 4.30 J/cm² @Temperature 23.0 °C | 20.5 ft-lb/in² @Temperature 73.4 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+11 ohm-cm @Thickness 0.750 mm | 1.00e+11 ohm-cm @Thickness 0.0295 in |
Dielectric Strength | 14.0 kV/mm @Thickness 1.00 mm | 356 kV/in @Thickness 0.0394 in |
Arc Resistance | 60 - 120 sec @Thickness 3.00 mm | 60 - 120 sec @Thickness 0.118 in |
Comparative Tracking Index | 525 V @Thickness 3.00 mm | 525 V @Thickness 0.118 in |
Hot Wire Ignition, HWI | 7.0 - 15 sec @Thickness 0.750 mm | 7.0 - 15 sec @Thickness 0.0295 in |
| 7.0 - 15 sec @Thickness 1.50 mm | 7.0 - 15 sec @Thickness 0.0591 in |
| 15 - 30 sec @Thickness 3.00 mm | 15 - 30 sec @Thickness 0.118 in |
High Amp Arc Ignition, HAI | >= 120 arcs @Thickness 0.750 mm | >= 120 arcs @Thickness 0.0295 in |
| >= 120 arcs @Thickness 1.50 mm | >= 120 arcs @Thickness 0.0591 in |
| >= 120 arcs @Thickness 3.00 mm | >= 120 arcs @Thickness 0.118 in |
High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80.0 mm/min | 1.00 - 3.15 in/min |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 86.0 µm/m-°C @Thickness 2.00 mm, Temperature 23.0 - 55.0 °C | 47.8 µin/in-°F @Thickness 0.0787 in, Temperature 73.4 - 131 °F |
CTE, linear, Transverse to Flow | 122 µm/m-°C @Thickness 2.00 mm, Temperature 23.0 - 55.0 °C | 67.8 µin/in-°F @Thickness 0.0787 in, Temperature 73.4 - 131 °F |
Melting Point | 260 °C | 500 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 202 °C | 396 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 69.0 °C | 156 °F |
UL RTI, Electrical | 130 °C @Thickness 0.750 mm | 266 °F @Thickness 0.0295 in |
| 130 °C @Thickness 1.50 mm | 266 °F @Thickness 0.0591 in |
| 130 °C @Thickness 3.00 mm | 266 °F @Thickness 0.118 in |
UL RTI, Mechanical with Impact | 75.0 °C @Thickness 0.750 mm | 167 °F @Thickness 0.0295 in |
| 75.0 °C @Thickness 1.50 mm | 167 °F @Thickness 0.0591 in |
| 75.0 °C @Thickness 3.00 mm | 167 °F @Thickness 0.118 in |
UL RTI, Mechanical without Impact | 110 °C @Thickness 0.750 mm | 230 °F @Thickness 0.0295 in |
| 110 °C @Thickness 1.50 mm | 230 °F @Thickness 0.0591 in |
| 110 °C @Thickness 3.00 mm | 230 °F @Thickness 0.118 in |
Flammability, UL94 | HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
Glow Wire Ignition Temperature | 725 °C @Thickness 3.00 mm | 1340 °F @Thickness 0.118 in |
| 750 °C @Thickness 0.750 mm | 1380 °F @Thickness 0.0295 in |
| 775 °C @Thickness 1.50 mm | 1430 °F @Thickness 0.0591 in |
Glow Wire Flammability Index | 700 °C @Thickness 3.00 mm | 1290 °F @Thickness 0.118 in |
| 725 °C @Thickness 0.750 mm | 1340 °F @Thickness 0.0295 in |
| 750 °C @Thickness 1.50 mm | 1380 °F @Thickness 0.0591 in |
|
Processing Properties | Metric | English | Comments |
---|
Rear Barrel Temperature | 280 - 310 °C | 536 - 590 °F |
Middle Barrel Temperature | 280 - 310 °C | 536 - 590 °F |
Front Barrel Temperature | 280 - 310 °C | 536 - 590 °F |
Nozzle Temperature | 280 - 310 °C | 536 - 590 °F |
Melt Temperature | 285 - 305 °C | 545 - 581 °F |
Mold Temperature | 65.0 - 95.0 °C | 149 - 203 °F |
Drying Temperature | 80.0 °C @Time 14400 sec | 176 °F @Time 4.00 hour |
|
Descriptive Properties |
---|
Agency Ratings | ASTM D4066 PA0161 |
| ASTM D6779 PA0161 |
Automotive Specifications | GM, GMW16447P-PA66-T1 |
| GM, QK 002921 E |
Suggested Max Regrind (%) | 25 |
Uses | Appliances |
| Automotive Applications |
| Connectors |
| Consumer Applications |
| Electrical/Electronic Applications |
| Fasteners |
| Gears |
| Industrial Applications |