MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow Nordel® IP 4725P High Hardness Extruded Profile
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Nordel® IP 4725P is a low viscosity semicrystalline grade which offers ease of processing, fast cure rates and high states of cure with standard sulfur cure systems. It is designed for molded and extruded applications requiring low viscosity, high green strength and high finished hardness. It is ideally suited for high hardness extruded profiles and molded goods. It can also be peroxide cured.

Information provided by manufacturer.

Key Words: 001166A06-4
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.283 g/cc
Mooney Viscosity 44
@Temperature 100 °C
ML 1 + 4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 90Vulcanizate, Press cured, TC95 +3min at 160°C
Hardness, Shore D 46Vulcanizate, Press cured, TC95 +3min at 160°C
Tensile Strength, Ultimate 15.13 MPaVulcanizate, Press cured, TC95 +3min at 160°C
Elongation at Break 213 %Vulcanizate, Press cured, TC95 +3min at 160°C
50% Modulus 0.00570 GPa
@Strain 50 %
Vulcanizate, Press cured, TC95 +3min at 160°C
100% Modulus 0.00843 GPa
@Strain 100 %
Vulcanizate, Press cured, TC95 +3min at 160°C
200% Modulus 0.01448 GPa
@Strain 200 %
Vulcanizate, Press cured, TC95 +3min at 160°C
Compression Set 53 %
@Temperature 100 °C
Pellets cured MDR TC95 + 15 min at 160°C, 22 hr at 100°C; Method B
 
Descriptive Properties
Formulation as Tested0.5ZnDBC
 0.5TMTD
 0.5DPTH
 1Stearic Acid
 1Vulkalent E/C
 1.5TBBS
 100Nordel® IP 4725P
 12Liquid BR (Ricon 153)
 15Paraffinic Oil
 5Zinc Oxide
 6Sulfur
 60Ground Calcium Carbonate
 60Precipitated Calcium Carbonate
 70N-550 Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow Nordel® IP 4725P Heat Resistant Molding
Dow Nordel® IP 4520 Molded Golf Grip
Dow Nordel® IP 4570 Radiator/Heater Hose
Dow Nordel® IP 4725P General Purpose Molding
Dow Nordel® NDR 4820P EPDM Hydrocarbon Rubber

PDVG26 / 34146

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.