MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ascend Performance Materials Vydyne® R535J NT0665 Nylon 66, 35% Glass Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Glass Fiber Filled

Material Notes: Vydyne R535J NT0665 is a natural, 35% glass-filled, high-flow PA66 resin that is heat-stabilized with an electrically neutral heat stabilizer. It is specially designed for electrical applications requiring high dielectric strength, low conductivity and corrosion resistance.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³DAM; ISO 1183
Water Absorption 0.80 %
@Time 86400 sec
0.80 %
@Time 24.0 hour
DAM; ISO 62
Moisture Absorption at Equilibrium 1.6 %1.6 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cm
@Thickness 2.00 mm
0.0040 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm
@Thickness 2.00 mm
0.0090 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 209 MPa30300 psiDAM; ISO 527-2
Elongation at Break 2.8 %2.8 %DAM; ISO 527-2
Tensile Modulus 11.6 GPa1680 ksiDAM; ISO 527-2
Flexural Strength 300 MPa43500 psiDAM; ISO 178
Flexural Modulus 10.5 GPa1520 ksiDAM; ISO 178
Poissons Ratio 0.400.40ISO 527-2
Izod Impact, Notched (ISO)  11.0 kJ/m²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 12.0 kJ/m²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
Charpy Impact Unnotched  6.80 J/cm²
@Temperature -30.0 °C
32.4 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
 7.90 J/cm²
@Temperature 23.0 °C
37.6 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched  1.10 J/cm²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm
@Thickness 1.00 mm
1.00e+14 ohm-cm
@Thickness 0.0394 in
DAM; IEC 60093
Dielectric Strength 20.0 kV/mm
@Thickness 1.00 mm
508 kV/in
@Thickness 0.0394 in
DAM; IEC 60243
Arc Resistance 120 - 180 sec
@Thickness 3.00 mm
120 - 180 sec
@Thickness 0.118 in
PLC 5; ASTM D 495
Comparative Tracking Index 600 V
@Thickness 3.00 mm
600 V
@Thickness 0.118 in
IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 15 - 30 sec15 - 30 secPLC 3; UL 746
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/min0.394 - 1.00 in/minPLC 1; UL 746
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 21.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
11.7 µin/in-°F
@Thickness 0.0787 in,
Temperature 95.0 - 131 °F
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 106 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
58.9 µin/in-°F
@Thickness 0.0787 in,
Temperature 73.4 - 131 °F
DAM; ISO 11359-2
Melting Point 260 °C500 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 261 °C502 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 251 °C484 °FUnannealed; DAM; ISO 75-2/A
UL RTI, Electrical  120 °C
@Thickness 0.750 mm
248 °F
@Thickness 0.0295 in
UL 746
 120 °C
@Thickness 1.50 mm
248 °F
@Thickness 0.0591 in
UL 746
 120 °C
@Thickness 3.00 mm
248 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical with Impact  100 °C
@Thickness 0.750 mm
212 °F
@Thickness 0.0295 in
UL 746
 100 °C
@Thickness 1.50 mm
212 °F
@Thickness 0.0591 in
UL 746
 105 °C
@Thickness 3.00 mm
221 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical without Impact  125 °C
@Thickness 0.750 mm
257 °F
@Thickness 0.0295 in
UL 746
 125 °C
@Thickness 1.50 mm
257 °F
@Thickness 0.0591 in
UL 746
 125 °C
@Thickness 3.00 mm
257 °F
@Thickness 0.118 in
UL 746
Flammability, UL94  HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Glow Wire Ignition Temperature  725 °C
@Thickness 1.50 mm
1340 °F
@Thickness 0.0591 in
IEC 60695-2-13
 750 °C
@Thickness 3.00 mm
1380 °F
@Thickness 0.118 in
IEC 60695-2-13
 775 °C
@Thickness 0.750 mm
1430 °F
@Thickness 0.0295 in
IEC 60695-2-13
Glow Wire Flammability Index  725 °C
@Thickness 1.50 mm
1340 °F
@Thickness 0.0591 in
IEC 60695-2-12
 750 °C
@Thickness 0.750 mm
1380 °F
@Thickness 0.0295 in
IEC 60695-2-12
 800 °C
@Thickness 3.00 mm
1470 °F
@Thickness 0.118 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Middle Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Front Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Nozzle Temperature 280 - 310 °C536 - 590 °FInjection
Melt Temperature 285 - 305 °C545 - 581 °FInjection
Mold Temperature 65.0 - 95.0 °C149 - 203 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 4.00 hour4.00 hourInjection
 
Descriptive Properties
AdditiveHeat Stabilizer
 Lubricant
Agency RatingsASTM, D4066 PA012G35
 ASTM, D6779 PA012G35
 EC, 1935/2004
 EU, 10/2011
 EU, 2023/2006
 FDA, 21 CFR 177.1500
AppearanceNatural Color
Automotive Material SpecificationDelphi M5600V
FeaturesChemical Resistant
 Corrosion Resistant
 Good Colorability
 Good Electrical Properties
 Good Mold Release
 High Flow
 High Strength
 Laser Markable
 Lubricated
 Organic Heat Stabilized
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific
UL File NumberE70062

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Barlog Plastics KEBATER BM240 PBT, 40% mineral reinforced, food grade
Barlog Plastics KEBATER BF230 PBT, 30% glass fiber reinforced, food grade
Gharda Chemicals G-PAEK™ 1230GF Ultra High Performance PEK Polymer
BASF Ultradur® B 4300 G6 FC 30% Glass Filled PBT
VICTREX™ PEEK 450CA20 Polyetheretherketone, 20% Carbon Fibre Reinforced

PASCE9831 / 220932

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.