MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Kinetics MIM F1537 (ASTM F1537) HIP and Heat Treat
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy; Cobalt Base

Material Notes: Most commonly used within the medical market on applications requiring these characteristics:
  • Bio-compatibility
  • Corrosion resistance
  • High strength
  • Nonmagnetic
  • Wear resistance.

Information provided by Kinetics, Inc.

Key Words: Metal Injection Molding
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.25 g/ccSintered (HIP)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 32
Tensile Strength, Ultimate 130 ksiAnnealed
 145 ksiHot-Worked
 160 ksiTypical
Tensile Strength, Yield 75.0 ksiAnnealed
 85.0 ksiTypical
 101 ksiHot-Worked
Elongation at Break 12 %in 1 inch Hot-Worked
 20 %in 1 inch Annealed
 27 %in 1 inch Typical
Reduction of Area 23 %
Charpy Impact, Unnotched 80.0 ft-lb1/2 size bar
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.10 - 0.35 %
Chromium, Cr 26 - 30 %
Cobalt, Co 58.40 - 68.9 %
Iron, Fe <= 0.75 %by difference
Manganese, Mn <= 1.0 %
Molybdenum, Mo 5.0 - 7.0 %
Nickel, Ni <= 1.0 %
Nitrogen, N <= 0.25 %
Silicon, Si <= 1.0 %
 
Descriptive Properties
Surface Finish40 Ra

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
PSM Industries PolyAlloys MIM-316L sintered Stainless Steel
Kinetics MIM 2.5% SiFe Soft Magnetic Steel
PSM Industries PolyAlloys MIM-2700 sintered Low Alloy Steel
Kinetics MIM 12 Chrome
Kinetics MIM F15 (Kovarâ„¢) Low CTE Alloy

NKINET15 / 138094

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.