MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes 214® alloy, sheet, 32 hours exposure at 870°C (1600°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Intended principally for use at temperatures of 955°C and above, exhibits resistance to oxidation that exceeds virtually all conventional heat-resistant wrought alloys. Applications include mesh belts, trays, and fixtures for firing of pottery and fine china, and the heat treatment of electronic devices and technical grade ceramics, used for foil construction honeycomb seals, combustor splash plates, and other static oxidation- limited parts, catalytic converter internals, burner cup material in auxiliary heaters for military vehicles, refractory anchors, furnace flame hoods, and rotary calciners for processing chloride compounds, and as hospital waste incinerator internals.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N07214, DIN 17744 No.2.4646
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.05 g/ccat RT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 965 MPa
Tensile Strength, Yield 565 MPa
@Strain 0.2 %
Elongation at Break 35 %in 50.8 mm
Modulus of Elasticity 218 GPaRT
 137 GPa
@Temperature 1000 °C
 151 GPa
@Temperature 900 °C
 162 GPa
@Temperature 800 °C
 170 GPa
@Temperature 700 °C
 177 GPa
@Temperature 600 °C
 184 GPa
@Temperature 500 °C
 190 GPa
@Temperature 400 °C
 199 GPa
@Temperature 300 °C
 204 GPa
@Temperature 200 °C
 210 GPa
@Temperature 100 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0001359 ohm-cmRT
 0.0001209 ohm-cm
@Temperature 1050 °C
 0.000121 ohm-cm
@Temperature 1100 °C
 0.0001216 ohm-cm
@Temperature 1000 °C
 0.0001219 ohm-cm
@Temperature 1150 °C
 0.0001229 ohm-cm
@Temperature 1200 °C
 0.0001249 ohm-cm
@Temperature 900 °C
 0.0001292 ohm-cm
@Temperature 800 °C
 0.0001337 ohm-cm
@Temperature 700 °C
 0.0001368 ohm-cm
@Temperature 600 °C
 0.0001369 ohm-cm
@Temperature 100 °C
 0.0001369 ohm-cm
@Temperature 200 °C
 0.0001369 ohm-cm
@Temperature 300 °C
 0.0001369 ohm-cm
@Temperature 300 °C
 0.0001377 ohm-cm
@Temperature 400 °C
 0.0001379 ohm-cm
@Temperature 500 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.3 µm/m-°C
@Temperature 25.0 - 200 °C
 13.6 µm/m-°C
@Temperature 25.0 - 300 °C
 14.1 µm/m-°C
@Temperature 25.0 - 400 °C
 14.6 µm/m-°C
@Temperature 25.0 - 500 °C
 15.2 µm/m-°C
@Temperature 25.0 - 600 °C
 15.8 µm/m-°C
@Temperature 25.0 - 700 °C
 16.6 µm/m-°C
@Temperature 25.0 - 800 °C
 17.6 µm/m-°C
@Temperature 25.0 - 900 °C
 18.6 µm/m-°C
@Temperature 25.0 - 1000 °C
Specific Heat Capacity 0.452 J/g-°CRT
 0.470 J/g-°C
@Temperature 100 °C
 0.493 J/g-°C
@Temperature 200 °C
 0.515 J/g-°C
@Temperature 300 °C
 0.538 J/g-°C
@Temperature 400 °C
 0.561 J/g-°C
@Temperature 500 °C
 0.611 J/g-°C
@Temperature 600 °C
 0.668 J/g-°C
@Temperature 700 °C
 0.705 J/g-°C
@Temperature 800 °C
 0.728 J/g-°C
@Temperature 900 °C
 0.742 J/g-°C
@Temperature 1000 °C
 0.749 J/g-°C
@Temperature 1100 °C
 0.753 J/g-°C
@Temperature 1200 °C
Thermal Conductivity 12.0 W/m-KRT
 12.8 W/m-K
@Temperature 100 °C
 14.2 W/m-K
@Temperature 200 °C
 15.9 W/m-K
@Temperature 300 °C
 18.4 W/m-K
@Temperature 400 °C
 21.1 W/m-K
@Temperature 500 °C
 23.9 W/m-K
@Temperature 600 °C
 26.9 W/m-K
@Temperature 700 °C
 29.7 W/m-K
@Temperature 800 °C
 31.4 W/m-K
@Temperature 900 °C
 34.0 W/m-K
@Temperature 1100 °C
 34.7 W/m-K
@Temperature 1000 °C
 36.7 W/m-K
@Temperature 1200 °C
Melting Point 1355 - 1400 °C
Solidus 1355 °C
Liquidus 1400 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 4.5 %
Boron, B <= 0.010 %
Carbon, C 0.050 %
Chromium, Cr 16 %
Iron, Fe 3.0 %
Manganese, Mn <= 0.50 %
Nickel, Ni 75 %
Silicon, Si <= 0.20 %
Yttrium, Y 0.010 %
Zirconium, Zr <= 0.10 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

NH21AW / 16419

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.