SABIC LNP™ THERMOCOMP™ Compound FX10009 Polyethylene, Unspecified (PE, Unspecified)
Categories:
Polymer
;
Thermoplastic
;
Polyethylene (PE)
Material Notes:
LNP THERMOCOMP FX10009 compound is based on Polyethylene (PE) resin containing proprietary fillers. Added features of this grade include: Improved Dielectric Properties.
Features: Dielectrics,Circuit Solution
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
2.50
g/cc
0.0903
lb/in³
ISO 1183
Water Absorption
0.080 %
@Time 86400 sec
0.080 %
@Time 24.0 hour
ISO 62-1
Moisture Absorption
0.0300 %
0.0300 %
Injection Molding
Viscosity
7.5
cP
@Load 10.0 kg,
Temperature 190 °C
7.5
cP
@Load 22.0 lb,
Temperature 374 °F
MVR cc/10 min; ISO 1133
12.5
cP
@Load 10.0 kg,
Temperature 220 °C
12.5
cP
@Load 22.0 lb,
Temperature 428 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow
0.015
-
0.020
cm/cm
0.015
-
0.020
in/in
SABIC method
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
20.0
MPa
2900
psi
5 mm/min; ISO 527
Elongation at Break
1.2 %
1.2 %
5 mm/min; ISO 527
Tensile Modulus
2.55
GPa
370
ksi
1 mm/min; ISO 527
Flexural Strength
15.0
MPa
2180
psi
break, 2mm/min; ISO 178
Flexural Modulus
2.75
GPa
399
ksi
2 mm/min; ISO 178
Izod Impact, Notched (ISO)
3.50
kJ/m²
1.67
ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
5.50
kJ/m²
2.62
ft-lb/in²
80*10*4; ISO 180/1U
Electrical Properties
Metric
English
Comments
Dielectric Constant
13.1
@Frequency 1e+9 Hz
13.1
@Frequency 1e+9 Hz
IEC 60250
13.4
@Frequency 5.00e+8 Hz
13.4
@Frequency 5.00e+8 Hz
IEC 60250
13.6
@Frequency 100000 Hz
13.6
@Frequency 100000 Hz
IEC 60250
Dissipation Factor
0.0080
@Frequency 5.00e+8 Hz
0.0080
@Frequency 5.00e+8 Hz
IEC 60250
0.0080
@Frequency 1e+9 Hz
0.0080
@Frequency 1e+9 Hz
IEC 60250
0.0090
@Frequency 1e+8 Hz
0.0090
@Frequency 1e+8 Hz
IEC 60250
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
130
µm/m-°C
@Temperature 23.0 - 60.0 °C
72.2
µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
CTE, linear, Transverse to Flow
150
µm/m-°C
@Temperature 23.0 - 60.0 °C
83.3
µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)
100
°C
212
°F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi)
60.0
°C
140
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
Processing Properties
Metric
English
Comments
Zone 2
200
-
210
°C
392
-
410
°F
Zone 3
205
-
215
°C
401
-
419
°F
Melt Temperature
210
-
215
°C
410
-
419
°F
Injection Molding
Mold Temperature
15.0
-
55.0
°C
59.0
-
131
°F
Drying Temperature
80.0
°C
176
°F
Injection Molding
Dry Time
4.00
hour
4.00
hour
Injection Molding
Back Pressure
0.200
-
0.300
MPa
29.0
-
43.5
psi
Screw Speed
30
-
60
rpm
30
-
60
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH81601 / 289548
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.