MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Gharda Chemicals G-PAEK™ 1230CF Ultra High Performance PEK Polymer
Categories: Polymer; Thermoplastic; Polyketone; Polyaryletherketone (PAEK), Carbon Fiber Filled

Material Notes: Product Details: Ultra High Performance Thermoplastic material, 30% carbon fiber reinforced in Poly Aryl Ether Ketone, semi-crystalline granules suitable for injection molding, easy flow, Black in color

Application Areas: Suitable for high temperature application, where higher strength & stiffness needed in load bearing application. Excellent wear resistance. Chemically resistant to aggressive environments, suitable for sterilization for medical and food contact applications.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.40 g/cc
Water Absorption 0.050 %
@Time 86400 sec
Linear Mold Shrinkage, Flow 0.0011 cm/cm410°C nozzle, 220°C mold
Linear Mold Shrinkage, Transverse 0.0080 cm/cm410°C nozzle, 220°C mold
Crystallinity 40 %DSC
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 108ASTM D785
Hardness, Shore D 91
Tensile Strength, Yield 75.0 MPa
@Temperature 250 °C
ASTM D638
 95.0 MPa
@Temperature 200 °C
ASTM D638
 125 MPa
@Temperature 150 °C
ASTM D638
 185 MPa
@Temperature 100 °C
ASTM D638
 250 MPa
@Temperature 23.0 °C
ASTM D638
 260 MPa
@Temperature -10.0 °C
ASTM D638
 275 MPa
@Temperature -50.0 °C
ASTM D638
Elongation at Break 2.0 %ASTM D638
Tensile Modulus 22.6 GPaASTM D638
Flexural Strength 360 MPaASTM D790
Flexural Modulus 22.0 GPaASTM D790
Izod Impact, Notched 50.0 J/mASTM D256
Izod Impact, Unnotched NBASTM D256
 
Thermal PropertiesOriginal ValueComments
Melting Point 370 - 372 °CDSC
Deflection Temperature at 1.8 MPa (264 psi) 368 °C
Glass Transition Temp, Tg 152 - 154 °CDSC/onset
Flammability, UL94 V-0
@Thickness 0.800 mm
 
Processing PropertiesOriginal ValueComments
Processing Temperature 390 - 425 °C
Nozzle Temperature 425 °C
Mold Temperature 200 - 220 °C
Drying Temperature 150 °C
Dry Time 4 - 6 hour
 
Descriptive Properties
Hopper/ Throat Temperature60-80°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Gharda Chemicals G-PAEK™ 1230FC Ultra High Performance PEK Polymer
Gharda Chemicals G-PAEK™ 1230GF Ultra High Performance PEK Polymer
EMS-Grivory Grivory® HT1V-3 FWA black 9225 PA6T/6I-GF30
Ensinger TECASINT 1011 Polyimide (PI)
Gharda Chemicals G-PAEK™ 1200G Ultra High Performance PEK Polymer

PGHARD993 / 108528

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.