MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

General Plastics LAST-A-FOAM® FR-10112 Foam
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane Foam, Unreinforced

Material Notes:

Information provided by General Plastics Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.192 g/cc0.00694 lb/in³ASTM D1622
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 1.88 MPa272 psiParallel to Rise; ASTM D1623
 1.89 MPa274 psiPerpendicular to Rise; ASTM D1623
Flexural Strength 3.15 MPa457 psiRise Parallel to Test Span; ASTM D790 Method 1-A
 3.19 MPa462 psiRise Parallel to Beam Thick.; ASTM D790 Method 1-A
Flexural Modulus 0.14907 GPa21.621 ksiRise Parallel to Test Span; ASTM D790 Method 1-A
 0.15499 GPa22.479 ksiRise Parallel to Beam Thick.; ASTM D790 Method 1-A
Compressive Strength  1.97 MPa
@Temperature 177 °C
285 psi
@Temperature 350 °F
Parallel to Rise; ASTM D1621
 2.50 MPa
@Temperature 177 °C
362 psi
@Temperature 350 °F
Perpendicular to Rise; ASTM D1621
 3.08 MPa
@Temperature 121 °C
446 psi
@Temperature 250 °F
Parallel to Rise; ASTM D1621
 3.31 MPa
@Temperature 121 °C
480 psi
@Temperature 250 °F
Perpendicular to Rise; ASTM D1621
 4.34 MPa
@Temperature 23.9 °C
630 psi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
 4.50 MPa
@Temperature 23.9 °C
652 psi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
Compressive Modulus  0.05317 GPa
@Temperature 177 °C
7.712 ksi
@Temperature 350 °F
Parallel to Rise; ASTM D1621
 0.06395 GPa
@Temperature 177 °C
9.275 ksi
@Temperature 350 °F
Perpendicular to Rise; ASTM D1621
 0.076511 GPa
@Temperature 121 °C
11.097 ksi
@Temperature 250 °F
Parallel to Rise; ASTM D1621
 0.077338 GPa
@Temperature 121 °C
11.217 ksi
@Temperature 250 °F
Perpendicular to Rise; ASTM D1621
 0.09984 GPa
@Temperature 23.9 °C
14.48 ksi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 0.1002 GPa
@Temperature 23.9 °C
14.54 ksi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
Poissons Ratio 0.300.30
 
Thermal PropertiesMetricEnglishComments
CTE, linear 37.8 µm/m-°C
@Temperature -28.9 - 71.1 °C
21.0 µin/in-°F
@Temperature -20.0 - 160 °F
GP Method
Thermal Conductivity 0.00591 W/m-K0.0410 BTU-in/hr-ft²-°F"K" Value; ASTM C518
 
Descriptive Properties
Tumbling Friability (%)20.420 minutes at 60 rpm; ASTM C421

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
General Plastics LAST-A-FOAM® FR-10108 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-10106 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-10115 Foam
Overview of materials for Thermoset Polyurethane Foam, Unreinforced
General Plastics LAST-A-FOAM® FR-10110 Polyurethane Foam

PGENR087 / 186873

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.