MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

E-Polymers TEKAMID® JN2 PPE+PA66 Un-reinforced Chemical resistance PA/PPE Alloy
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Polyphenylene Ether/PPO

Material Notes: Polyamide (Nylon) Resin. TEKAMID is widely being used in manufacturing of automotive and industrial parts with its outstanding mechanical, thermal and chemical properties.

JN-series: PA66/PPE, PA6/PPE alloy (Unreinforced, GF reinforced, MF reinforced)

Information Provided by E-Polymers Co., Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.13 g/cc1.13 g/ccASTM D792
Water Absorption 0.50 %
@Time 86400 sec
0.50 %
@Time 24.0 hour
Linear Mold Shrinkage 0.017 cm/cm0.017 in/in
Linear Mold Shrinkage, Transverse 0.013 cm/cm0.013 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 66.708 MPa9675.2 psiASTM D638
Elongation at Break 50 %50 %ASTM D638
Flexural Strength 99.08 MPa14370 psiASTM D790
Flexural Modulus 2.374 GPa344.3 ksiASTM D790
Izod Impact, Notched 1.67 J/cm3.12 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 204 °C399 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 125 °C257 °FASTM D648
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Melt Temperature 260 - 290 °C500 - 554 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
E-Polymers TEKAMID® JN1 PPE+PA66 Un-reinforced High flow Heat resistance PA/PPE Alloy
Polygon Composites PolyMed® CW Circumferential Fiber Engineered Composite Orientation Medical Tubing
BLUESTAR LXS 315 PPE-PS
BLUESTAR LXS 312 PPE-HIPS, 20% Mineral Filled
BLUESTAR LXS 109 PPE-PS

PEPOLZ007 / 103504

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.