MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics FireMaster® Marine Plus blanket Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Manufactured from FireMaster® Plus fibre, FireMaster® Marine Plus blanket is a highly insulating blanket especially developed for fire protection applications that are very space or weight sensitive.

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Absorption Coefficient 0.15
@Frequency 125 Hz
sound, 45mm x64kg/m3, no surface covering material used, class A; BS EN ISO 354-2003
 0.40
@Frequency 125 Hz
sound, 45mm x64kg/m3, face with glass cloth, class B; BS EN ISO 354-2003
 0.45
@Frequency 4000 Hz
sound, 45mm x64kg/m3, face with30µm reinforced Al foil, class C; BS EN ISO 354-2003
 0.45
@Frequency 125 Hz
sound, 45mm x64kg/m3, face with30µm reinforced Al foil, class C; BS EN ISO 354-2003
 0.65
@Frequency 4000 Hz
sound, 45mm x64kg/m3, face with glass cloth, class B; BS EN ISO 354-2003
 0.65
@Frequency 1000 Hz
sound, 45mm x64kg/m3, face with30µm reinforced Al foil, class C; BS EN ISO 354-2003
 0.65
@Frequency 2000 Hz
sound, 45mm x64kg/m3, face with30µm reinforced Al foil, class C; BS EN ISO 354-2003
 0.75
@Frequency 4000 Hz
sound, 45mm x64kg/m3, no surface covering material used, class A; BS EN ISO 354-2003
 0.75
@Frequency 500 Hz
sound, 45mm x64kg/m3, face with30µm reinforced Al foil, class C; BS EN ISO 354-2003
 0.75
@Frequency 250 Hz
sound, 45mm x64kg/m3, no surface covering material used, class A; BS EN ISO 354-2003
 0.80
@Frequency 2000 Hz
sound, 45mm x64kg/m3, face with glass cloth, class B; BS EN ISO 354-2003
 0.85
@Frequency 1000 Hz
sound, 45mm x64kg/m3, face with glass cloth, class B; BS EN ISO 354-2003
 0.90
@Frequency 250 Hz
sound, 45mm x64kg/m3, face with30µm reinforced Al foil, class C; BS EN ISO 354-2003
 0.95
@Frequency 250 Hz
sound, 45mm x64kg/m3, face with glass cloth, class B; BS EN ISO 354-2003
 0.95
@Frequency 500 Hz
sound, 45mm x64kg/m3, face with glass cloth, class B; BS EN ISO 354-2003
 1.0
@Frequency 500 Hz
sound, 45mm x64kg/m3, no surface covering material used, class A; BS EN ISO 354-2003
 1.0
@Frequency 1000 Hz
sound, 45mm x64kg/m3, no surface covering material used, class A; BS EN ISO 354-2003
 1.0
@Frequency 2000 Hz
sound, 45mm x64kg/m3, no surface covering material used, class A; BS EN ISO 354-2003
 
Mechanical PropertiesOriginal ValueComments
Sound Insulation 22.4 dB
@Frequency 100 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 23.3 dB
@Frequency 125 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 24 dB
@Frequency 100 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 25.5 dB
@Frequency 125 Hz
45mm x 128kg/m3 attached to 5mm steel substrate; ISO 140/3
 25.7 dB
@Frequency 160 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 26 dB
@Frequency 125 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 26.1 dB
@Frequency 125 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 28 dB
@Frequency 100 Hz
45mm x 128kg/m3 attached to 5mm steel substrate; ISO 140/3
 28.4 dB
@Frequency 200 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 28.6 dB
@Frequency 160 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 28.8 dB
@Frequency 160 Hz
45mm x 128kg/m3 attached to 5mm steel substrate; ISO 140/3
 29.1 dB
@Frequency 200 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 29.2 dB
@Frequency 100 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 30.3 dB
@Frequency 200 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 30.4 dB
@Frequency 250 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 30.5 dB
@Frequency 160 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 31.8 dB
@Frequency 250 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 36.6 dB
@Frequency 250 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 36.9 dB
@Frequency 315 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 37.9 dB
@Frequency 200 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 39 dB
@Frequency 315 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 39.7 dB
@Frequency 315 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 40.7 dB
@Frequency 400 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 43.6 dB
@Frequency 400 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 43.9 dB
@Frequency 400 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 44.3 dB
@Frequency 250 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 44.6 dB
@Frequency 500 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 44.8 dB
@Frequency 2000 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 45.2 dB
@Frequency 315 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 46 dB
@Frequency 2500 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 46.9 dB
@Frequency 500 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 47.4 dB
@Frequency 1600 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 48 dB
@Frequency 400 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 48 dB
@Frequency 500 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 48.5 dB
@Frequency 630 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 49.1 dB
@Frequency 1250 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 49.2 dB
@Frequency 3150 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 50.1 dB
@Frequency 2000 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 51.2 dB
@Frequency 2500 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 51.5 dB
@Frequency 1000 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 51.5 dB
@Frequency 630 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 51.6 dB
@Frequency 630 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 52.2 dB
@Frequency 500 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 52.2 dB
@Frequency 800 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 52.7 dB
@Frequency 800 Hz
50mm x 48kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 53.1 dB
@Frequency 1600 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 53.1 dB
@Frequency 3150 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 55.1 dB
@Frequency 1250 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 55.8 dB
@Frequency 800 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 56 dB
@Frequency 1000 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 56.3 dB
@Frequency 630 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 57.1 dB
@Frequency 1000 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 57.6 dB
@Frequency 2500 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 58.3 dB
@Frequency 3150 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 58.8 dB
@Frequency 800 Hz
75mm x 64kg/m3 attached to 6mm stiffened steel bulkhead with steel; EN ISO 10140-2
 59 dB
@Frequency 1250 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 60.3 dB
@Frequency 1000 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 60.4 dB
@Frequency 2500 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 60.9 dB
@Frequency 1600 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 61.8 dB
@Frequency 4000 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 62 dB
@Frequency 2000 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 62.1 dB
@Frequency 3150 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 62.5 dB
@Frequency 1250 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 63.8 dB
@Frequency 1600 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 64.5 dB
@Frequency 2000 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 64.5 dB
@Frequency 5000 Hz
45mmx64kg/m3 attached to 5mm steel substrate; ISO 140/3
 65 dB
@Frequency 4000 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 66.5 dB
@Frequency 5000 Hz
45mmx128kg/m3 attached to 5mm steel substrate; ISO 140/3
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.0272 W/m-K
@Temperature -50.0 °C
at 128 kg/m3; ASTM C177-10
 0.0313 W/m-K
@Temperature 0.000 °C
at 128 kg/m3; ASTM C177-10
 0.0367 W/m-K
@Temperature 38.0 °C
at 128 kg/m3; ASTM C177-10
 0.0429 W/m-K
@Temperature 100 °C
at 128 kg/m3; ASTM C177-10
 0.0499 W/m-K
@Temperature 150 °C
at 128 kg/m3; ASTM C177-10
 0.0500 W/m-K
@Temperature 200 °C
at 128 kg/m3; ASTM C201
 0.0500 W/m-K
@Temperature 200 °C
at 96kg/m3; ASTM C201
 0.0561 W/m-K
@Temperature 200 °C
at 128 kg/m3; ASTM C177-10
 0.0600 W/m-K
@Temperature 200 °C
at 64kg/m3; ASTM C201
 0.0800 W/m-K
@Temperature 400 °C
at 128 kg/m3; ASTM C201
 0.100 W/m-K
@Temperature 400 °C
at 96kg/m3; ASTM C201
 0.110 W/m-K
@Temperature 400 °C
at 64kg/m3; ASTM C201
 0.120 W/m-K
@Temperature 600 °C
at 128 kg/m3; ASTM C201
 0.150 W/m-K
@Temperature 600 °C
at 96kg/m3; ASTM C201
 0.170 W/m-K
@Temperature 600 °C
at 64kg/m3; ASTM C201
 0.180 W/m-K
@Temperature 800 °C
at 128 kg/m3; ASTM C201
 0.210 W/m-K
@Temperature 800 °C
at 96kg/m3; ASTM C201
 0.250 W/m-K
@Temperature 1000 °C
at 128 kg/m3; ASTM C201
 0.260 W/m-K
@Temperature 800 °C
at 64kg/m3; ASTM C201
 0.290 W/m-K
@Temperature 1000 °C
at 96kg/m3; ASTM C201
 0.380 W/m-K
@Temperature 1000 °C
at 64kg/m3; ASTM C201
Insulation R Value 0.78
@Thickness 25.0 mm
at ambient temp @ 48kg/m3
 0.78
@Thickness 25.0 mm
at ambient temp @ 64kg/m3
 0.93
@Thickness 30.0 mm
at ambient temp @ 48kg/m3
 0.94
@Thickness 30.0 mm
at ambient temp @ 64kg/m3
 1.09
@Thickness 35.0 mm
at ambient temp @ 64kg/m3
 1.09
@Thickness 35.0 mm
at ambient temp @ 48kg/m3
 1.25
@Thickness 40.0 mm
at ambient temp @ 48kg/m3
 1.25
@Thickness 40.0 mm
at ambient temp @ 64kg/m3
 1.387
@Thickness 60.0 mm
at ambient temp @ 48kg/m3
 1.56
@Thickness 50.0 mm
at ambient temp @ 64kg/m3
 1.56
@Thickness 50.0 mm
at ambient temp @ 48kg/m3
 1.88
@Thickness 60.0 mm
at ambient temp @ 64kg/m3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

CMORF6424 / 203208

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.