MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zytel® BM73G15THS BK317 PA6-IGF15
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled

Material Notes: 15% Glass Reinforced, Heat Stabilized, Polyamide 6

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccDAM; ISO 1183
Water Absorption 7.5 %
@Thickness 2.00 mm
DS; DAM; Sim. to ISO 62
Moisture Absorption 2.60 %
@Thickness 2.00 mm
DS; DAM; Sim. to ISO 62
Viscosity 300000 cP
@Shear Rate 1000 1/s,
Temperature 280 °C
Melt; ISO 11443
Linear Mold Shrinkage, Flow 0.0070 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.012 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 180 MPaH 961/30; DAM; ISO 2039-1
Tensile Strength at Break 65.0 MPa50% RH; ISO 527-1/-2
 100 MPaDAM; ISO 527-1/-2
Elongation at Break 5.0 %DAM; ISO 527-1/-2
 23 %50% RH; ISO 527-1/-2
Tensile Modulus 2500 MPa50% RH; ISO 527-1/-2
 5000 MPaDAM; ISO 527-1/-2
Poissons Ratio 0.35DAM
 0.3850% RH
Izod Impact, Notched (ISO) 11.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 11.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 21.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 28.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched 80.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 110 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eU
Charpy Impact, Notched 11.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 12.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 13.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 21.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 29.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmDAM; IEC 62631-3-1
Dissipation Factor 0.016
@Frequency 1e+6 Hz
DAM; IEC 62631-2-1
 0.016
@Frequency 100 Hz
DAM; IEC 62631-2-1
Comparative Tracking Index 600 VDAM; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 221 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 190 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 10.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 60.0 °C10°C/min; DAM; ISO 11357-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Oxygen Index 25 %DAM; ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 235 - 250 °CRange, Extrusion
 255 - 265 °CRange, Blow Molding
 260 °COptimum, Blow Molding
 270 °COptimum, Injection
 260 - 280 °CRange, Injection
Mold Temperature 90.0 °COptimum, Blow Molding
 80.0 - 110 °CRange, Blow Molding
 70.0 - 120 °CInjection
 100 °COptimum, Injection
Drying Temperature 80.0 °CInjection
 80.0 °CExtrusion
 110 - 120 °CBlow Molding
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
 4.00 - 6.00 hourBlow Molding, Dehumidified Dryer
 4.00 - 6.00 hourExtrusion, Dehumidified Dryer
Moisture Content <= 0.030 %Blow Molding
 <= 0.060 %Extrusion
 <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaRange, Injection
 
Descriptive Properties
AdditivesRelease agent
Drying RecommendedyesBlow Molding
 yesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
ISO designationISO 16396-PA6-I,GF15,M1CGHR,S14-050
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>PA6-IGF15<ISO 11469
PolymerPA6-GF15
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPA6-IGF15ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Nypel® RC6024 BK 30% Mineral/Glass Filled PA6 (Dry)
DuPont Mobility and Materials Zytel® BM73G15P BK317 PA6-IGF15
DuPont Mobility and Materials Zytel® 70G25HSL NC010 PA66-GF25
Celanese Zytel® ST811HS NC010 PA6-HI
Celanese Zytel® 74G33J NC010 PA66+PA6-GF33

PDSX5388 / 198028

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.