MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Assab Steels ASSAB XW-41 Cold Work Steel
Categories: Metal; Ferrous Metal; Carbon Steel; High Carbon Steel; Chrome-moly Steel; Tool Steel; Cold Work Steel

Material Notes: XW-41 is a high-carbon, high chromium tool steel alloyed with molybdenum and vanadium characterized by:
  • High wear resistance
  • High compressive strength
  • Good through-hardening properties
  • High stability in hardening
  • Good resistance to tempering-back.

XW-41 is used when cutting thicker, harder materials; when forming with tools subjected to bending stresses and where high impact loads are involved. XW-41 can be supplied in various finishes, including the hot-rolled, pre-machined and fine machined condition. It is also available in the form of hollow bar and rings.

AISI D2, W.-Nr. 1.2379

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.277 lb/in³
 0.275 lb/in³
@Temperature 400 °C
 0.276 lb/in³
@Temperature 200 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 411020°C Austenitizing temperature, for tempering at 650°C
 441050°C Austenitizing temperature, for tempering at 650°C
 551020°C Austenitizing temperature, for tempering at 550°C
 571050°C Austenitizing temperature, for tempering at 400°C
 591020°C Austenitizing temperature, for tempering at 400°C
 601050°C Austenitizing temperature, for tempering at 200°C
 61At 980°C during hardening, soaking time 30 minutes
 621050°C Austenitizing temperature, for tempering at 550°C
 62Hardened and tempered.
 62.5At 980°C during hardening, soaking time 60 minutes
 631020°C Austenitizing temperature, for tempering at 200°C
 64.25At 1060°C during hardening, soaking time 30 minutes
 65At 1020°C during hardening, soaking time 30 minutes
 65.5At 1020°C during hardening, soaking time 60 minutes
Modulus of Elasticity 193 GPa
 173 GPa
@Temperature 400 °C
Compressive Strength 1900 MPaHRC 55 Rc0.2
 2200 MPaHRC 62 Rc0.2.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µm/m-°C
@Temperature 20.0 - 200 °C
 13.4 µm/m-°C
@Temperature 20.0 - 400 °C
Specific Heat Capacity 0.110 BTU/lb-°F
@Temperature 20.0 °C
Thermal Conductivity 20.0 W/m-K
@Temperature 20.0 °C
 21.0 W/m-K
@Temperature 200 °C
 23.0 W/m-K
@Temperature 400 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 1.55 %
Chromium, Cr 11.8 %
Iron, Fe 84.35 %
Manganese, Mn 0.40 %
Molybdenum, Mo 0.80 %
Silicon, Si 0.30 %
Vanadium, V 0.80 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Assab Steels ASSAB XW-42 Cold Work Steel
Assab Steels ASSAB XW-5 Cold Work Steel
AISI Type A2 Tool Steel
AISI Type O1 Oil-hardening Tool Steel, oil quenched at 800°C, tempered at 425°C
AISI 1045 Steel, Quenched and Tempered to 390 HB

NASSAB04 / 15022

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.