MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AGC Fluon® C-55AP ETFE
Categories: Polymer; Thermoplastic; Fluoropolymer; ETFE/ECTFE; Fluorocarbon ETFE/ECTFE, Molded/Extruded

Material Notes: Description: Fluon® ETFE is a melt-processable copolymer of tetrafluoroethylene and ethylene. Fluon ETFE possesses a unique combination of desirable properties such as higher resistance to heat and chemical attack and outstanding physical toughness. It is processable by conventional extrusion, injection molding, roto-molding, roto-lining, and electrostatic coating. It is available in a variety of forms including 1/8” pellets, designated as ‘P’, and powder, designated as ‘B’.

Benefits:

  • High resistance to heat: Fluon ETFE has a continuous use temperature of 150°C.
  • Excellent chemical resistance
  • Outstanding physical toughness: Fluon ETFE has better physical properties than most other fluoropolymers.
  • Low smoke and flame characteristics: Fluon ETFE is rated 94 V-0 by Underwriters Laboratories Inc.
  • Outstanding resistance to weather and aging
  • Good dielectric properties
  • Non-stick characteristics
Applications:
  • Wire & cable (automotive, industrial, aerospace, transit, and appliance markets)
  • Film and sheets
  • Tubing and pipe
  • Electronic components
  • Electrostatic and roto-molded vessel linings
  • Valves, fittings, and pump housings

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.74 g/ccASTM D792
Water Absorption >= 0.030 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.018 cm/cm
Melt Flow 3.9 - 6.5 g/10 min
@Load 5.00 kg,
Temperature 297 °C
ASTM D3159
Melt Index of Compound 1.0 - 2.0 g/10 min
@Load 0.160 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 67
Tensile Strength at Break 10.0 MPa
@Temperature 175 °C
 20.0 MPa
@Temperature 140 °C
 30.0 MPa
@Temperature 100 °C
 40.0 MPa
@Temperature 60.0 °C
 50.0 MPa
@Temperature 40.0 °C
Tensile Strength 7.00 MPa
@Temperature 200 °C
ASTM D638
 52.0 MPa
@Temperature 23.0 °C
ASTM D638
Tensile Strength, Yield 5.00 MPa
@Treatment Temp. 190 °C
 10.0 MPa
@Treatment Temp. 110 °C
 15.0 MPa
@Treatment Temp. 80.0 °C
 20.0 MPa
@Treatment Temp. 50.0 °C
 25.0 MPa
@Treatment Temp. 20.0 °C
Elongation at Break 382 %
@Temperature 23.0 °C
ASTM D638
 620 %
@Temperature 200 °C
ASTM D638
 400 %
@Treatment Temp. 10.0 °C
 500 %
@Treatment Temp. 50.0 °C
 600 %
@Treatment Temp. 90.0 °C
 700 %
@Treatment Temp. 110 °C
 700 %
@Treatment Temp. 175 °C
Flexural Strength 26.0 MPaASTM D790
 5.00 MPa
@Temperature 150 °C
 10.0 MPa
@Temperature 90.0 °C
 15.0 MPa
@Temperature 55.0 °C
 20.0 MPa
@Temperature 45.0 °C
Flexural Modulus 960 MPaASTM D790
 100 MPa
@Temperature 120 °C
 300 MPa
@Temperature 60.0 °C
 600 MPa
@Temperature 45.0 °C
 900 MPa
@Temperature 30.0 °C
Flex Crack Resistance 50000Cycles per MIT Folding Endurance; ASTM D2176
Izod Impact, Notched NBASTM D256
 NBASTM C256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+17 ohm-cmASTM D257
Dielectric Constant 2.6
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 1800 V/mil10 mil film; ASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 93.0 µm/m-°CASTM D696
Specific Heat Capacity 1.26 J/g-°C
Melting Point 265 °C
Maximum Service Temperature, Air 150 °C
Deflection Temperature at 0.46 MPa (66 psi) 115 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °CASTM D648
Brittleness Temperature -125 °CASTM D764
Flammability, UL94 V-0
Oxygen Index 32 %ASTM D2863
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 280 - 300 °C
Middle Barrel Temperature 270 - 290 °C
Front Barrel Temperature 260 - 280 °C
Nozzle Temperature 290 - 320 °C
Mold Temperature 60.0 - 120 °C
Injection Velocity 1.00 - 15.0 mm/sec
Injection Pressure 50.0 - 120 MPa
 
Descriptive Properties
Heat of Combustion5900 BTU/lbASTM D240

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Daikin NEOFLON® AP-210 PFA
Daikin NEOFLON® NP-101 FEP
AGC Fluon® C-88AXMP ETFE
AGC Fluon® C-88AP ETFE
Daikin NEOFLON® EP-521 Extrusion Grade ETFE

PAGCX014 / 191123

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.