MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Constellium PLAN 6061 Aluminum Rolled Plate
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Rolled plates in 6061 PLAN are optimized for minimum residual stress and improved dimensional tolerances. 6061 PLAN is mainly used for medium stressed mechanical components, manufactured by intensive machining. Typical applications include parts for printing and packaging machines, as well as conveying systems

Information provided by manufacturer

Key Words: EN AW-6061 T651
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.70 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 100
@Thickness 4.00 - 8.00 mm
 100
@Thickness 8.00 - 25.0 mm
 100
@Thickness 60.0 - 150 mm
 105
@Thickness 25.0 - 60.0 mm
Tensile Strength >= 275 MPa
@Thickness 100 - 150 mm
Temper T651; Standard EN 485-2
 >= 290 MPa
@Thickness 3.90 - 6.00 mm
Temper T651; Standard EN 485-2
 >= 290 MPa
@Thickness 6.00 - 12.5 mm
Temper T651; Standard EN 485-2
 >= 290 MPa
@Thickness 12.5 - 40.0 mm
Temper T651; Standard EN 485-2
 >= 290 MPa
@Thickness 40.0 - 80.0 mm
Temper T651; Standard EN 485-2
 >= 290 MPa
@Thickness 80.0 - 100 mm
Temper T651; Standard EN 485-2
 320 MPa
@Thickness 4.00 - 8.00 mm
Typical Strength; Standard EN 485-2
 320 MPa
@Thickness 60.0 - 150 mm
Typical Strength; Standard EN 485-2
 325 MPa
@Thickness 8.00 - 25.0 mm
Typical Strength; Standard EN 485-2
 330 MPa
@Thickness 25.0 - 60.0 mm
Typical Strength; Standard EN 485-2
Tensile Strength, Yield >= 240 MPa
@Strain 0.2 %,
Thickness 3.90 - 6.00 mm
Temper T651; Standard EN 485-2
 >= 240 MPa
@Strain 0.2 %,
Thickness 6.00 - 12.5 mm
Temper T651; Standard EN 485-2
 >= 240 MPa
@Strain 0.2 %,
Thickness 12.5 - 40.0 mm
Temper T651; Standard EN 485-2
 >= 240 MPa
@Strain 0.2 %,
Thickness 40.0 - 80.0 mm
Temper T651; Standard EN 485-2
 >= 240 MPa
@Strain 0.2 %,
Thickness 80.0 - 100 mm
Temper T651; Standard EN 485-2
 >= 240 MPa
@Strain 0.2 %,
Thickness 100 - 150 mm
Temper T651; Standard EN 485-2
 285 MPa
@Strain 0.2 %,
Thickness 4.00 - 8.00 mm
Typical Strength; Standard EN 485-2
 285 MPa
@Strain 0.2 %,
Thickness 60.0 - 150 mm
Typical Strength; Standard EN 485-2
 295 MPa
@Strain 0.2 %,
Thickness 8.00 - 25.0 mm
Typical Strength; Standard EN 485-2
 295 MPa
@Strain 0.2 %,
Thickness 25.0 - 60.0 mm
Typical Strength; Standard EN 485-2
Elongation at Break >= 5.0 %
@Thickness 80.0 - 100 mm
Temper T651; Standard EN 485-2
 >= 5.0 %
@Thickness 100 - 150 mm
Temper T651; Standard EN 485-2
 >= 6.0 %
@Thickness 40.0 - 80.0 mm
Temper T651; Standard EN 485-2
 >= 8.0 %
@Thickness 12.5 - 40.0 mm
Temper T651; Standard EN 485-2
 >= 9.0 %
@Thickness 6.00 - 12.5 mm
Temper T651; Standard EN 485-2
 >= 10 %
@Thickness 3.90 - 6.00 mm
Temper T651; Standard EN 485-2
 11 %
@Thickness 60.0 - 150 mm
Typical Elongation; Standard EN 485-2
 12 %
@Thickness 8.00 - 25.0 mm
Typical Elongation; Standard EN 485-2
 12 %
@Thickness 25.0 - 60.0 mm
Typical Elongation; Standard EN 485-2
 15 %
@Thickness 4.00 - 8.00 mm
Typical Elongation; Standard EN 485-2
Modulus of Elasticity 69.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000380 - 0.00000430 ohm-cmTemper T651
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.4 µm/m-°C
@Temperature 20.0 - 100 °C
Thermal Conductivity 150 - 170 W/m-KTemper T651
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 96.15 - 98.61 %as balance
Chromium, Cr 0.040 - 0.35 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Zinc, Zn <= 0.25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Alclad Aluminum 6061-O
Aluminum 6061-O
Aluminum 6061-T4; 6061-T451
Alclad Aluminum 6061-T6, T651

NCONS004 / 160267

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.