MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics IFB Structural TJM ™28 Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Manufacturing method: extrusion. These products offer superior performance in load bearing applications and in conditions where abrasion from mechanical and chemical abuse or flow of hot gases is severe. Our Structural Range of IFB deliver big energy savings for many markets and our global manufacturing footprint enables Morgan to meet your regional and global application demands.

Applications: Hot face refractory lining or as back-up insulation in:

  • Petrochemical (kilns, flues, refining vessels and heaters and reactor chambers)
  • Iron and steel industry (heat treatment and galvanising)
  • Coke and iron making (blast furnaces, hot blast stoves, hot blast and bustle main)
  • Ceramic industry (including kilns for domestic use)
  • Glass industry
  • Power generation

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.900 g/ccASTM C-133
Deformation 0.20 %
@Temperature 1320 °C,
Time 5400 sec
0.069 MPa; ASTM C-16
 
Mechanical PropertiesOriginal ValueComments
Modulus of Rupture 0.00180 GPaASTM C-133
Compressive Strength 2.50 MPaCold Crushing Strength; ASTM C-133
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.320 W/m-K
@Temperature 200 °C
ASTM C-182
 0.330 W/m-K
@Temperature 400 °C
ASTM C-182
 0.340 W/m-K
@Temperature 600 °C
ASTM C-182
 0.370 W/m-K
@Temperature 800 °C
ASTM C-182
 0.410 W/m-K
@Temperature 1000 °C
ASTM C-182
 0.460 W/m-K
@Temperature 1200 °C
ASTM C-182
Shrinkage 0.70 %
@Treatment Temp. 1510 °C,
Time 86400 sec
ASTM C-210
 
Component Elements PropertiesOriginal ValueComments
Al2O3 65 %
CaO 0.20 %
Fe2O3 0.70 %
K2O+Na2O 0.80 %
MgO 0.10 %
SiO2 32 %
TiO2 0.40 %
 
Descriptive Properties
Classification Temperature (°C)1540
Reversible Linear Expansion (%)0.8

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

CMORF6204 / 202988

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.