MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Monprene® CP-18178 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene CP-18178 is a high performance thermoplastic elastomer designed for a variety of consumer product applications requiring a soft, rubber-like feel. Monprene CP-18178 is a high hardness grade that exhibits sunlight resistance and UV absorbing characteristics, suitable for injection molding.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: High Flow; Light Stabilized; Low Density; Low Specific Gravity; Lubricated; Slip; High Hardness; Sunlight Resistant; UV Absorbing; Without Fillers

Uses: Consumer Applications; Handles; Kitchenware; Safety Equipment; Sporting Goods; Writing Instruments

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.890 g/cc0.0322 lb/in³ASTM D792
Melt Flow 17 g/10 min
@Load 2.16 kg,
Temperature 190 °C
17 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  78
@Time 5.00 sec
78
@Time 0.00139 hour
Injection Molded; ASTM D2240
 80
@Time 1.00 sec
80
@Time 0.000278 hour
Injection Molded; ASTM D2240
Tensile Strength at Break 9.03 MPa1310 psi20 in/min, Across Flow; ASTM D412
 9.38 MPa1360 psi20 in/min, Flow; ASTM D412
Tensile Stress at Strain  4.63 MPa
@Strain 100 %
672 psi
@Strain 100 %
20 in/min, Across Flow; ASTM D412
 5.87 MPa
@Strain 300 %
852 psi
@Strain 300 %
20 in/min, Across Flow; ASTM D412
 6.36 MPa
@Strain 100 %
922 psi
@Strain 100 %
20 in/min, Flow; ASTM D412
 7.86 MPa
@Strain 300 %
1140 psi
@Strain 300 %
20 in/min, Flow; ASTM D412
Elongation at Break 470 %470 %20 in/min, Flow; ASTM D412
 580 %580 %20 in/min, Across Flow; ASTM D412
Tear Strength 51.0 kN/m291 pli20 in/min, Across Flow; ASTM D624
 55.6 kN/m317 pli20 in/min, Flow; ASTM D624
Compression Set 28 %
@Temperature 22.8 °C,
Time 79200 sec
28 %
@Temperature 73.0 °F,
Time 22.0 hour
Type 1; ASTM D395B
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 182 - 232 °C360 - 450 °F
Middle Barrel Temperature 188 - 238 °C370 - 460 °F
Front Barrel Temperature 193 - 243 °C380 - 470 °F
Nozzle Temperature 199 - 249 °C390 - 480 °F
Melt Temperature 199 - 249 °C390 - 480 °F
Mold Temperature 35.0 - 48.9 °C95.0 - 120 °F
Injection Pressure 1.38 - 5.52 MPa200 - 800 psi
Back Pressure 0.172 - 0.689 MPa25.0 - 100 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
AppearanceNatural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ0794 / 237285

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.