MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Murtfeldt Murflor® Polytetrafluoroethylene
Categories: Polymer; Thermoplastic; Fluoropolymer; Polytetrafluoroethylene (PTFE); Polytetrafluoroethylene (PTFE), Extruded

Material Notes: Murflor® materials are suited to use in applications that require an excellent resistance to chemicals and heating steam. Murflor®’s working range starts at -200°C and can extend to +260°C with no mechanical load. Murflor® also has the lowest dynamic friction coefficient of all thermoplastics.

Special Properties:
• Best dynamic friction properties of all thermoplastics
• No stick/slip effect
• Very good anti-adhesion properties
• Electrically isolating
• Very high resistance to chemicals
• Very high resistance to hydrolysis
• Very tough, even at low temperatures
• Approved for use in the food industry (FDA

Information provided by Murtfeldt Kunststoffe GmbH & Co. KG.

Key Words: PTFE
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.18 g/ccISO 1183-1
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 58DIN 53505
Tensile Strength, Yield 20.0 MPaISO 527-1/-2
Elongation at Break 300 %ISO 527-1/-2
Modulus of Elasticity 0.750 GPa
Compressive Yield Strength 4.50 MPa
@Strain 1 %
dry; ISO 604
Charpy Impact Unnotched NBISO 179
Charpy Impact, Notched 16.0 kJ/m²ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.080
Sand Slurry 21µm/km
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+17 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohmIEC 60093
Dielectric Constant 2.0
@Frequency 100 Hz
IEC 60250
 2.1
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 20.0 kV/mmIEC 60243-1
Dielectric Loss Index 0.00010
@Frequency 1e+6 Hz
IEC 60250
 0.00030
@Frequency 100 Hz
IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear 160 µm/m-°C
@Temperature 23.0 - 100 °C
Melting Point 321 °CISO 11357-1
Maximum Service Temperature, Air 260 °C
@Time 7.20e+7 sec
 300 °C
@Time <=86400 sec
Minimum Service Temperature, Air -200 °C
Glass Transition Temp, Tg 127 °CISO 11357-1
Flammability, UL94 V-0
 
Compliance PropertiesOriginal ValueComments
FDA Yes
 
Descriptive Properties
ColorNatural

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Murtfeldt Murflor® Polytetrafluoroethylene, 25% Carbon
Murtfeldt Murflor® + Bronze Polytetrafluoroethylene, 60% Bronze
Overview of materials for Polytetrafluoroethylene (PTFE), Extruded
Chemours Teflon® PTFE 6C Resin for Lubricated Paste Extrusion
Guarniflon PTFE G200 Polytetrafluoroethylene

PMURT934 / 156581

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.