MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Crucible Steel CPM® S110V® Stainless Tool Steel
Categories: Metal; Ferrous Metal; Martensitic; Stainless Steel; Tool Steel

Material Notes: CPM S110V is a high alloy martensitic stainless tool steel produced by the Crucible Particle Metallurgy (CPM) process. CPM S110V contains a high volume fraction of both vanadium-rich and niobium-rich primary alloy carbides for exceptionally good wear resistance compared to other commercially available PM tool steels. It also offers better corrosion resistance than 440C or CPM S90V.

CPM S110V is available on special request in the as-HIP condition or as a clad layer on components. It is not available in forged or rolled bar lengths.

The CPM process results in a fine and uniform carbide distribution in CPM S110V compared to conventionally produced high alloy tool steels which results in relatively good machining, grinding, and toughness characteristics despite the high alloy content.

Information provided by Crucible Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  47.5
@Tempering Temp. 649 °C
47.5
@Tempering Temp. 1200 °F
austenitized at 2150°F then quenched and tempered
 53.5
@Tempering Temp. 593 °C
53.5
@Tempering Temp. 1100 °F
austenitized at 2150°F then quenched and tempered
 58.5
@Tempering Temp. 566 °C
58.5
@Tempering Temp. 1050 °F
austenitized at 2150°F then quenched and tempered
 60
@Tempering Temp. 260 °C
60
@Tempering Temp. 500 °F
austenitized at 2150°F then quenched and tempered
 60.5
@Tempering Temp. 399 °C
60.5
@Tempering Temp. 750 °F
austenitized at 2150°F then quenched and tempered
 60.5
@Tempering Temp. 551.7 °C
60.5
@Tempering Temp. 1025 °F
austenitized at 2150°F then quenched and tempered
 61.5
@Tempering Temp. 538 °C
61.5
@Tempering Temp. 1000 °F
austenitized at 2150°F then quenched and tempered
 63.5
@Tempering Temp. 524 °C
63.5
@Tempering Temp. 975 °F
austenitized at 2150°F then quenched and tempered
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 2.8 %2.8 %
Chromium, Cr 15.25 %15.25 %
Cobalt, Co 2.5 %2.5 %
Iron, Fe 65.2 %65.2 %as balance
Molybdenum, Mo 2.25 %2.25 %
Niobium, Nb (Columbium, Cb) 3.0 %3.0 %
Vanadium, V 9.0 %9.0 %
 
Descriptive Properties
Corrosion Rate0 mm/yr at 500°Fin dilute aqua regia
 1 mm/yr at 750°Fin dilute aqua regia
 7 mm/yr at 1025°Fin dilute aqua regia
 9 mm/yr at 975°Fin dilute aqua regia
Pitting Resistance-150 mVpolarization curves in 5% NaCl, tempered at 1025°F
 200 mVpolarization curves in 5% NaCl, tempered at 500°F
Wear Resistance29 mgweight loss, 63 HRC
 45 mgweight loss, 60 HRC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Crucible Steel CPM® S35VN™ Stainless Steel
Carpenter Pyrowear® 675 Stainless Steel, Tempered 510°C, Longitudinal Properties
Crucible Steel CPM® S90V® (420V®) Tool Steel
ATI Allegheny Ludlum Stainless Steel Type 301, 1/2 Hard (UNS S30100)
Carpenter Pyrowear® 675 Stainless Steel, Tempered 316°C, Longitudinal Properties

NCRUC904 / 160355

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.