MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Mitsubishi Hostaphan® RN, 19 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Unreinforced

Material Notes: Hostaphan® RN is a transparent, biaxially oriented film made of polyethylene terephthalate (PET) and characterized by outstanding physical properties. Hostaphan® RN is the standard product for the following applications:
  • Films for packaging
    • Coating
    • Laminating
    • Metallizing
    • Printing
  • Decorative films
  • Gloss laminations
  • Adhesive tapes
  • Insulation tapes
  • Release
    • Transfer film
    • Release film for thermosetting resings
  • Hot stamping/Roll leaf

Information provided by Mitsubishi Polyester Film

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.40 g/cc
@Temperature 23.0 °C
ASTM D1505-68, method C
Linear Mold Shrinkage 0.013 cm/cm
@Time 900 sec
DIN 40634
Linear Mold Shrinkage, Transverse 0.0010 cm/cm
@Time 900 sec
DIN 40634
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 230 MPaTest speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Film Tensile Strength at Yield, TD 260 MPaTest speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Film Elongation at Break, MD >= 110 %Test speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Film Elongation at Break, TD 100 %Test speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Modulus of Elasticity 4.40 GPa
@Temperature 23.0 °C
MD; Test speed 1%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
 5.00 GPa
@Temperature 23.0 °C
TD; Test speed 1%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Coefficient of Friction, Static 0.40DIN 53375 or ASTM D1894
 
Optical PropertiesOriginal ValueComments
Haze 6.0 %Enlarged measurement angle; ASTM D1003-61, method A
Transmission, Visible 90 %transparent; thickness not quantified
 
Descriptive Properties
F5-value (MPa)105ISO 527-1, ISO 527-3; Sample type 2; TD; Test speed 100%/min.; 23ºC, 50% r.h.
 110ISO 527-1, ISO 527-3; Sample type 2; MD; Test speed 100%/min.; 23ºC, 50% r.h.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsubishi Hostaphan® RN, 15 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Mitsubishi Hostaphan® RN, 12 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Mitsubishi Hostaphan® RN, 30 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Mitsubishi Hostaphan® RN, 36 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Mitsubishi Hostaphan® RN, 50 micron Nominal Thickness Universal Polyethylene Terephthalate Film

PMUE029 / 108410

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.