System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Aurora Plastics TufTech™ SE11-023E PVC Compound
Categories:
Polymer
;
Thermoplastic
;
Vinyl (PVC)
Material Notes:
Application: Automotive – PVC, black, exterior weatherable, elastomeric, extrusion molding compound.
Information provided by S&E Specialty Polymers; S&E Specialty Polymers was aquired by Aurora Plastics in 2017.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Specific Gravity
<=
1.22
g/cc
ISO 1183
Mechanical Properties
Original Value
Comments
Hardness, Shore A
55 - 65
@Time 15.0 sec
ISO 868
58.6 - 69.3
@Treatment Temp. 85.0 °C,
Time 605000 sec
Heat Aging; ISO 188, Method B
Tensile Strength at Break
1890
psi
500mm/min; ISO 527, 1A
1950
psi
@Treatment Temp. 85.0 °C,
Time 605000 sec
Heat Aging; ISO 188, Method B
Elongation at Break
385 %
500mm/min; ISO 527, 1A
394 %
@Treatment Temp. 85.0 °C,
Time 605000 sec
Heat Aging; ISO 188, Method B
Tear Strength
>=
188
pli
Method B, angle die, 500mm/min.; ISO 34-1
Compression Set
25 %
@Temperature 24.0 °C,
Time 259000 sec
ISO 815-1, Type A
57 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815-1, Type A
Thermal Properties
Original Value
Comments
Minimum Service Temperature, Air
-34.0
°C
Cold Flex; No cracks; SAE J323, Method A
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
PSEPN044 / 179048
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.