MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Rogers Corporation RT/duroid® 6006 Ceramic-PTFE Composite Microwave Laminate
Categories: Polymer; Thermoplastic; Fluoropolymer; Polytetrafluoroethylene (PTFE); Polytetrafluoroethylene (PTFE), Glass Filled, Molded

Material Notes: Features:
  • High dielectric constant for circuit size reduction
  • Low loss - Ideal for operating at X-band or below
  • Tight dielectric constant and thickness control for repeatable circuit performance
  • Low moisture absorption. Reduces effects of moisture on electrical loss
  • Cladding - EDC or rolled copper foil, also thick aluminum, brass or copper plate (one side)
  • Lead-free process compatible

Typical Applications:

  • Space Saving Circuitry
  • Patch Antennas
  • Ground Radar Warning Systems
  • Satellite Communications Systems
  • Power Amplifiers
  • Aircraft Collision Avoidance Systems

Information provided by Rogers Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.70 g/ccASTM D792
Moisture Absorption at Equilibrium 0.050 %
@Temperature 50.0 °C,
Time 173000 sec
0.05 in.; IPC-TM-650 2.6.2.1
Thickness 5.00 - 100 milRange of Standard Thicknesses
Deformation 0.33 %
@Pressure 7.00 MPa,
Temperature 50.0 °C
Z direction; 24 hrs; ASTM D621
 2.1 %
@Pressure 7.00 MPa,
Temperature 150 °C
Z direction; 24 hrs; ASTM D621
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 17.0 MPaY direction; 0.1/min strain rate; ASTM D638
 20.0 MPaX direction; 0.1/min strain rate; ASTM D638
Elongation at Break 4.0 - 6.0 %Y direction; 0.1/min strain rate; ASTM D638
 12 - 13 %X direction; 0.1/min strain rate; ASTM D638
Tensile Modulus 517 ksiY direction; 0.1/min strain rate; ASTM D638
 627 ksiX direction; 0.1/min strain rate; ASTM D638
Flexural Strength 38.0 MPaCondition A; ASTM D790
Flexural Modulus 1951 MPaY direction, Condition A; ASTM D790
 2634 MPaX direction, Condition A; ASTM D790
Compressive Yield Strength 54.0 MPa
@Strain 33 %
Z direction; 0.05/min strain rate; ASTM D695
Compressive Modulus 1069 MPaZ direction; 0.05/min strain rate; ASTM D695
Peel Strength 14.3 pliCopper, after solder float; IPC-TM-650 2.4.8
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.00e+13 ohm-cmCondition A; IPC 2.5.17.1
Surface Resistance 7.00e+13 ohmCondition A; IPC 2.5.17.1
Dielectric Constant 6.0 - 6.3
@Frequency 1e+10 Hz
Process, Clamped stripline, Z-direction; IPC-TM-650 2.5.5.5
 6.45
@Frequency 8.00e+9 - 4.00e+10 Hz
Design, Z-direction; Differential Phase Length Method
Dissipation Factor 0.0027
@Frequency 1e+10 Hz
Z direction; IPC-TM-650 2.5.5.5
 
Thermal PropertiesOriginal ValueComments
CTE, linear 34.0 µm/m-°C
@Temperature 0.000 - 100 °C
Y-Direction; 5°C/min; ASTM D3386
 47.0 µm/m-°C
@Temperature 0.000 - 100 °C
X-Direction; 5°C/min; ASTM D3386
 117 µm/m-°C
@Temperature 0.000 - 100 °C
Z-Direction; 5°C/min; ASTM D3386
Specific Heat Capacity 0.970 J/g-°Ccalculated
Thermal Conductivity 0.490 W/m-K
@Temperature 80.0 °C
ASTM C518
Decomposition Temperature 500 °CTGA; ASTM D3850
Flammability, UL94 V-0
 
Descriptive Properties
Thermal Coefficient of Dielectric Constant-410 ppm/°CIPC-TM-650 2.5.5.5; 10 GHz; -50°C to 170°C; Z-Direction

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Rogers Corporation RT/duroid® 6010.2LM Ceramic-PTFE Composite Microwave Laminate
Overview of materials for Polytetrafluoroethylene (PTFE), Glass Filled, Molded
Rogers Corporation RT/duroid® 5880LZ Lightweight, High Frequency PTFE Laminate
Rogers Corporation RO3730 Antenna Grade Laminate
Rogers Corporation RT/duroid® 5870 Glass Microfiber Reinforced PTFE High Frequency Laminate

PROGA974 / 138414

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.