MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Avient Dynaflex™ G7690-1 (Natural) Thermoplastic Elastomer (TPE)
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Dynaflex™ G7690-1 (Natural) is an easy processing, general purpose TPE designed for a wide variety of applications, including those where FDA compliance is required. - Overmold Adhesion to Polypropylene - Rubbery Feel - Soft Touch

Color concentrates with polypropylene (PP), ethylene vinyl acetate (EVA), or low density polyethylene (PE) carriers are most suitable for coloring Dynaflex™ G7690-1 (Natural). Improved color dispersion can be achieved by using higher melt flow concentrates (with a melt flow from 25 - 40 g/10 min). Typical loadings for color concentrates are 1% to 5% by weight. Liquid color can be used, but mineral oil based carriers may have a significant effect on the final hardness value. Concentrates based on PVC should not be used. A high color match consistency can be obtained by using precolored compounds available from GLS. The final determination of color concentrate suitability should be determined by customer trials. Purge thoroughly before and after use of this product with a low flow (0.5 - 2.5 MFR) polyethylene (PE) or polypropylene (PP). Regrind levels up to 20% can be used with Dynaflex™ G7690-1 (Natural) with minimal property loss, provided that the regrind is free of contamination. To minimize losses during molding, the melt temperature should remain as low as possible. The final determination of regrind effectiveness should be determined by the customer. Dynaflex™ G7690-1 (Natural) has excellent melt stability. Maximum residence times may vary, depending on the size of the barrel. Generally, the barrel should be emptied if it is idle for periods of 8 - 10 minutes or longer. Drying is not Required Injection Speed: 1 to 3 in/sec 1st Stage - Boost Pressure: 350 to 900 psi 2nd Stage - Hold Pressure: 30% of Boost Hold Time (Thick Part): 3 to 10 sec Hold Time (Thin Part): 1 to 3 sec

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/ccASTM D792
Viscosity 14300 cP
@Shear Rate 11200 1/s,
Temperature 200 °C
ASTM D3835
 74000 cP
@Shear Rate 1340 1/s,
Temperature 200 °C
ASTM D3835
Linear Mold Shrinkage, Flow 0.0060 - 0.014 cm/cmASTM D955
Melt Flow 14 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 8910 sec; ASTM D2240
Tensile Strength at Break 11.0 MPa
@Temperature 23.0 °C
Die C2 hr; ASTM D412
Tensile Stress at Strain 4.55 MPa
@Strain 100 %,
Temperature 23.0 °C
Die C2 hr; ASTM D412
 6.21 MPa
@Strain 300 %,
Temperature 23.0 °C
Die C2 hr; ASTM D412
Elongation at Break 600 %
@Temperature 23.0 °C
Die C2 hr; ASTM D412
Tear Strength 46.4 kN/mASTM D624
Compression Set 38 %
@Temperature 23.0 °C,
Time 79200 sec
ASTM D395B
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 166 - 177 °C
Middle Barrel Temperature 177 - 193 °C
Front Barrel Temperature 188 - 227 °C
Nozzle Temperature 193 - 227 °C
Mold Temperature 15.6 - 37.8 °C
Back Pressure 0.000 - 0.827 MPa
Screw Speed 40 - 100 rpm
 
Compliance PropertiesOriginal ValueComments
FDA Yes21 CFR 177.1210
 
Descriptive Properties
AppearanceNatural Color
FeaturesGeneral Purpose
 Good Colorability
 Good Flow
 Good Processability
 Good Processing Stability
FormsPellets
Generic MaterialTPE
Generic NameThermoplastic Elastomer (TPE)
Processing MethodInjection Molding
Regional AvailabilityAsia Pacific
RoHS ComplianceRoHS Compliant
Suggested Max Regrind20%
UsesConsumer Applications
 Flexible Grips
 Gaskets
 General Purpose
 Overmolding
 Seals
 Sporting Goods

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Avient Dynaflex™ G2701-1000-02 Thermoplastic Elastomer (TPE)
Avient Dynaflex™ D3226-1000-03 Thermoplastic Elastomer (TPE)
Avient Dynaflex™ G2706-1000-00 Thermoplastic Elastomer (TPE)
Avient Dynaflex™ G2703-1000-00 Thermoplastic Elastomer (TPE)
Avient Dynaflex™ G7431-1001-00 Thermoplastic Elastomer (TPE)

PH0POL1194 / 145763

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.