MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AK Steel 444 Ferritic Stainless steel
Categories: Metal; Ferrous Metal; Ferritic; Stainless Steel; T 400 Series Stainless Steel

Material Notes: AK Steel 444 is a low-carbon, low nitrogen, ferritic stainless steel that provides pitting and crevice corrosion resistance superior to most ferritic stainless steels. Applications requiring superior corrosion resistance and resistance to chloride stress corrosion cracking are ideal for this alloy. Current uses include food processing, brewery and wine-making equipment; hot-water tanks and heat exchanger tubing and automotive components.

Information provided by AK Steel

Key Words: UNS S44400
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.75 g/cc0.280 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B <= 90<= 90
Tensile Strength, Ultimate >= 414 MPa>= 60000 psi
Tensile Strength, Yield 360 MPa
@Strain 0.2 %
52200 psi
@Strain 0.2 %
Elongation at Break >= 20 %>= 20 %in 2 inches
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000570 ohm-cm0.0000570 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 11.0 µm/m-°C
@Temperature 0.000 - 100 °C
6.11 µin/in-°F
@Temperature 32.0 - 212 °F
Specific Heat Capacity 0.427 J/g-°C
@Temperature 0.000 - 100 °C
0.102 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 26.8 W/m-K
@Temperature 100 °C
186 BTU-in/hr-ft²-°F
@Temperature 212 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.025 %<= 0.025 %
Chromium, Cr 17.5 - 19.5 %17.5 - 19.5 %
Iron, Fe >= 74.105 %>= 74.105 %As Remainder
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 1.75 - 2.5 %1.75 - 2.5 %
Nickel, Ni <= 1.0 %<= 1.0 %
Other, total 0.20 - 0.80 %0.20 - 0.80 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
444 Ferritic Stainless Steel, 18Cr-2Mo (UNS S44400)
ATI Allegheny Ludlum AL 444™ Ferritic Stainless Steel
AK Steel 439 Ferritic Stainless steel
Universal Wire Works Inconel 625 (AMS 5837) Filler Metal
Overview of materials for T 400 Series Stainless Steel

NAKS100 / 14703

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.