MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC XENOY™ X4870HH PC+PBT (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Unreinforced

Material Notes: XENOY X4870HH is a high heat, very high modulus and ductile PC/PET blend. Furthermore this resin provides chemical resistance, very low creep, low CTE, excellent fatique and high heat dimensional stability. The X4870HH could be positioned for body panels, housings, medical device enclosures, outdoor sports equipment.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.34 g/ccASTM D792
Density 1.34 g/ccISO 1183
Water Absorption 0.42 %23°C/sat; ISO 62
Moisture Absorption 0.140 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 7.0 g/10 min
@Load 5.00 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
 8.0 g/10 min
@Load 5.00 kg,
Temperature 266 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 105 MPaISO 2039-1
Tensile Strength at Break 45.0 MPa5 mm/min; ASTM D638
 45.0 MPa50 mm/min; ISO 527
 45.0 MPa5 mm/min; ISO 527
 50.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 61.0 MPa5 mm/min; ASTM D638
 63.0 MPa5 mm/min; ISO 527
 65.0 MPa50 mm/min; ASTM D638
 67.0 MPa50 mm/min; ISO 527
Elongation at Break 10 %50 mm/min; ISO 527
 10 %5 mm/min; ISO 527
 30 %50 mm/min; ASTM D638
 60 %5 mm/min; ASTM D638
Elongation at Yield 3.3 %50 mm/min; ASTM D638
 3.6 %5 mm/min; ISO 527
 3.7 %5 mm/min; ASTM D638
 3.8 %50 mm/min; ISO 527
Tensile Modulus 4300 MPa1mm/min; ISO 527
 4600 MPa5 mm/min; ASTM D638
Flexural Yield Strength 98.0 MPa2 mm/min; ISO 178
 104 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 4000 MPa2 mm/min; ISO 178
 4250 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 90.0 J/mASTM D256
 70.0 J/m
@Temperature -30.0 °C
ASTM D256
 80.0 J/m
@Temperature 0.000 °C
ASTM D256
Izod Impact, Notched (ISO) 10.0 kJ/m²80*10*4; ISO 180/1A
 6.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NB80*10*4; ISO 180/1U
Charpy Impact Unnotched NBEdgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 11.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 60.0 JASTM D3763
 60.0 J
@Temperature -20.0 °C
ASTM D3763
Impact Test 90.0 JMultiaxial Impact; ISO 6603
Taber Abrasion, mg/1000 Cycles 30CS-17, 1 kg; SABIC method
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 43.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 48.0 µm/m-°C
@Temperature -30.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 64.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 68.0 µm/m-°C
@Temperature -30.0 - 80.0 °C
ISO 11359-2
Thermal Conductivity 0.200 W/m-KISO 8302
Deflection Temperature at 0.46 MPa (66 psi) 131 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 132 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 113 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 113 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 137 °CRate B/50; ASTM D1525
 137 °CRate B/50; ISO 306
 139 °CRate B/120; ISO 306
 
Processing PropertiesOriginal ValueComments
Processing Temperature 60.0 - 80.0 °CHopper Temperature
Nozzle Temperature 260 - 275 °CInjection Molding
Zone 1 240 - 270 °C
Zone 2 250 - 275 °C
Zone 3 260 - 280 °C
Melt Temperature 265 - 275 °C
Mold Temperature 60.0 - 100 °C
Drying Temperature 110 - 120 °CInjection Molding
Dry Time 4.00 - 6.00 hourInjection Molding
Moisture Content 0.020 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10858 / 244325

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.