MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

(Viewing data as-entered. Click here to return)
Dow Dow™ DMDA-8007 HEALTH+™ HDPE
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE)

Material Notes: Product Description: Dow DMDA-8007 HEALTH+™ is a narrow molecular weight distribution high density homopolymer designed to offer excellent stiffness, low warpage, good toughness, and good moldability. The resin is suitable for injection –molded medical devices such as IV kit components and respiratory care as well as caps and closures for pharmaceutical packaging.
Main Characteristics:
  • Excellent stiffness
  • Low warpage
  • Good toughness
  • High gloss parts
Complies with: US FDA 21 CFR 177.1520©2.2; Canadian HPFB No Objection; EU, No 10/2011; USP XXII Class VI; Drug Master File Listing. Consult the regulations for complete details.

Availability: North America

Additive: Antiblock: No; Processing Aid: No; Slip: No

Agency Ratings: DMF; EU No 10/2011; FDA 21 CFR 177.1520© 2.2; HPFB (Canada) No Objection; USP XXIII, Class VI

Form: Pellets

Processing Method: Injection Molding

Information provided by The Dow Chemical Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.967 g/ccASTM D792
Melt Flow 8.3 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 180 g/10 min
@Load 21.6 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 61ASTM D2240
Tensile Strength at Break 2600 psiASTM D638
Tensile Strength, Yield 4500 psiASTM D638
Elongation at Break 350 %ASTM D638
Elongation at Yield 6.0 %ASTM D638
Flexural Modulus 205000 psi2% Secant; ASTM D790B
Tensile Impact Strength 80.0 ft-lb/in²Type S; ASTM D1822
 
Thermal PropertiesOriginal ValueComments
Melting Point 271 °F
Crystallization Temperature 248 °F
Deflection Temperature at 0.46 MPa (66 psi) 183 °FUnannealed; ASTM D648
Vicat Softening Point 268 °FASTM D1525
Brittleness Temperature <= -105 °FASTM D746

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDOWF441 / 311134

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.