MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Oxygen-free silver-bearing Copper, UNS C10400, OSO50 Temper flat products, rod, shapes, tubing
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold workability; good forgeability. Fabricated by coining, coppersmithing, drawing and upsetting, hot forging and pressing, spinning, swaging, stamping.

Applications: auto gaskets, radiators, busbars, conductivity wire, contacts, radio parts, winding, switches, terminals, commutator segments, chemical process equipment, printing rolls, clad metals, printed circuit foil.

Test specimens: flat products - 6mm thick, rod - 25mm OD, shapes - 13mm section, and tubing - 25mm OD x 1.65mm wall thickness.

Similar alloys distinguished only by silver content: 8 oz/ton Ag (UNS C10400), 10 oz/ton Ag (UNS C10500), 25 oz/ton Ag (UNS C10700).

Key Words: AMSIL Copper; Oxygen-free Silver-Copper; ASTM-B-152, QQ-C-502, QQ-C-576
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.94 g/ccUNS C10700
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell F 40
Tensile Strength, Ultimate 220 MPa
Tensile Strength, Yield 69.0 MPa
Elongation at Break 45 %Tubing
 50 %in 50 mm, flat products, shapes
 55 %Rod
Modulus of Elasticity 115 GPa
Poissons Ratio 0.307
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %
Shear Modulus 44.0 GPa
Shear Strength 150 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000172 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°C
@Temperature 20.0 - 100 °C
 17.3 µm/m-°C
@Temperature 20.0 - 200 °C
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.385 J/g-°C
Thermal Conductivity 388 W/m-K
@Temperature 20.0 °C
Melting Point <= 1083 °C
Solidus 1083 °C
Liquidus 1083 °C
Annealing Point >= 900 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 475 - 750 °C
Hot-Working Temperature 750 - 875 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu >= 99.95 %Includes Ag
Silver, Ag >= 0.027 %Min 8 troy oz./ton

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Oxygen-free silver-bearing Copper, UNS C10400, OSO25 Temper flat products, tubing
Oxygen-free Electronic Copper (OFE), UNS C10100, OS050 temper, flat products, rod, tubing, and shapes
Chicago Extruded Metals BioBrass® UNS C64700 Copper-Silicon Alloy
Electrolytic tough pitch anneal resistant Copper, UNS C11100
Copper, UNS C12100

MC10400b2 / 10416

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.