MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sibur BK-1675M Butyl Rubber (IIR)
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: EXXON Butyl 268, PB 301 Bayer. For general and medical goods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Mooney Viscosity 35 - 47
@Temperature 100 °C
ML 1-4
Ash <= 0.35 %
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break >= 19.0 MPa
Tensile Strength, Yield >= 7.00 MPa
Elongation at Break >= 600 %
 
Descriptive Properties
Loss During Drying<0.4%
Mass Share Adigol-20.05-0.2%
Mass Share Agidol-10.2-0.4%
Mass Share Anox-200.02-0.08%
Mass Share BC-30A0.1-0.5%
Mass Share Irganox-10100.02-0.08%
Mass Share of Calcium Stearate<1.2%
Mass Share of Iron<0.02%
Spread Flow Batch Error<±8 %
Unsaturation1.4-1.8%, mol

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Trelleborg T528 Butyl Rubber
ATG s.r.l. IIR Butyl Rubber
Butyl Rubber (IIR, CIIR, BIIR)
Sibur BK-1675N Butyl Rubber (IIR)
Trelleborg T641 Butyl Rubber

PSIB085 / 67648

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.