MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Copper Zinc Alloy, UNS C69220, H01 Temper, Flat Products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: 1/4 Hard

Typical uses: Automotive Parts; Electronic parts; Drinking water Fixtures, Plumbing

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.30 g/cc0.300 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers >= 140
@Load 0.500 kg
>= 140
@Load 1.10 lb
Tensile Strength 565 - 586 MPa82000 - 85000 psi
 579 MPa84000 psiTypical
Tensile Strength, Yield >= 317 MPa>= 46000 psi0.5% Ext
 331 MPa48000 psi0.5% Ext, Typical
Tensile Modulus 103 GPa14900 ksi
Modulus of Rigidity 42.00 GPa6092 ksi
Poissons Ratio 0.320.32
Machinability 78 %78 %
Forgeability 95 %95 %
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000180 ohm-cm0.0000180 ohm-cm9.5% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear  18.61 µm/m-°C
@Temperature 20.0 - 100 °C
10.34 µin/in-°F
@Temperature 68.0 - 212 °F
 18.61 µm/m-°C
@Temperature 20.0 - 200 °C
10.34 µin/in-°F
@Temperature 68.0 - 392 °F
Specific Heat Capacity 0.372 J/g-°C0.0890 BTU/lb-°F
Thermal Conductivity 2.597 W/m-K18.02 BTU-in/hr-ft²-°F
Melting Point 866.7 - 870.0 °C1592 - 1598 °F
Solidus 866.7 °C1592 °F
Liquidus 870.0 °C1598 °F
Annealing Point >= 520 °C>= 968 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature >= 410 °C>= 770 °FStress Relief
Solution Temperature >= 780.0 °C>= 1436 °F
Hot-Working Temperature >= 620.0 °C>= 1148 °F
Precipitation Temperature >= 500 °C>= 932 °F
 
Component Elements PropertiesMetricEnglishComments
Antimony, Sb <= 0.10 %<= 0.10 %
Copper, Cu 69 - 71 %69 - 71 %
Iron, Fe <= 0.10 %<= 0.10 %
Lead, Pb <= 0.080 %<= 0.080 %
Manganese, Mn 0.80 - 1.8 %0.80 - 1.8 %
Nickel, Ni <= 0.20 %<= 0.20 %
Phosphorus, P 0.050 - 0.20 %0.050 - 0.20 %
Silicon, Si 1.8 - 2.6 %1.8 - 2.6 %
Tin, Sn <= 0.30 %<= 0.30 %
Zinc, Zn 23.7 - 28.4 %23.7 - 28.4 %As Balance
 
Descriptive Properties
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC69220x1 / 292362

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.