MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Wolf Kunststoff ZEDEX® ZX-750V5KF 055 Fiber Reinforced Polymer Alloy
Categories: Polymer; Thermoplastic

Material Notes: Stiff; High elongation and yield stress; Low thermal expansion; Impact resistant
Applications: Textile Machinery; Compressors; Hinges; Handling; Machine Tools; Automotive Technology

Information provided by Zedex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.53 g/cc0.0553 lb/in³ISO 1183
Water Absorption 0.20 %
@Temperature 23.0 °C
0.20 %
@Temperature 73.4 °F
RMC 93%; DIN EN ISO 62
Moisture Absorption at Equilibrium 0.40 %0.40 %DIN EN ISO 62
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A >= 100>= 100DIN 53505
Hardness, Shore D 9090DIN 53505
Ball Indentation Hardness 160 MPa23200 psiDIN 2039
Tensile Strength at Break 93.1 MPa13500 psiDIN EN ISO 527
Tensile Strength 93.1 MPa13500 psiDIN EN ISO 527
Tensile Strength, Yield 61.0 MPa8850 psiElastic Limit
Tensile Stress at Strain 44.0 MPa
@Strain 1 %,
Time 3.60e+6 sec
6380 psi
@Strain 1 %,
Time 1000 hour
DIN 53444
Elongation at Break 6.8 %6.8 %DIN EN ISO 527
Elongation at Yield 2.4 %2.4 %Elastic Yield Point
 6.8 %6.8 %Elongation at Maximum Force; DIN EN ISO 527
Tensile Modulus 2.48 GPa360 ksiDIN EN ISO 527
Flexural Strength 177 MPa25700 psiOuter Fiber Stress at 3.5% Outer Fiber Strain; DIN EN ISO 178
 182 MPa26400 psiDIN EN ISO 178
 182 MPa26400 psiDIN EN ISO 178
Flexural Modulus 8.83 GPa1280 ksiDIN EN ISO 178
Flexural Strain at Break 6.8 %6.8 %DIN EN ISO 178
Flexural Strain at Yield 4.3 %4.3 %DIN EN ISO 178
Compressive Strain at Break 10.9 %10.9 %Nominal Compressive Strain at Compressive Strength; DIN EN ISO 604
 10.9 %10.9 %Nominal; DIN EN ISO 604
Compressive Yield Strength 101 MPa14600 psiElastic Limit
Compressive Strength 147 MPa21300 psiDIN EN ISO 604
 147 MPa21300 psibreak; DIN EN ISO 604
 61.0 MPa
@Time 3.60e+7 sec
8850 psi
@Time 10000 hour
 95.0 MPa
@Time 360000 sec
13800 psi
@Time 100 hour
 108 MPa
@Time 36.0 sec
15700 psi
@Time 0.0100 hour
 83.0 MPa
@Strain 3.5 %
12000 psi
@Strain 3.5 %
DIN EN ISO 604
Compressive Modulus 4.95 GPa718 ksiDIN EN ISO 604
Fatigue Strength 55.0 MPa
@# of Cycles 1.00e+6
7980 psi
@# of Cycles 1.00e+6
1 Hz
K Factor (ISO)  0.10 µm/km
@Temperature 20.0 °C
0.10 µm/km
@Temperature 68.0 °F
 0.70 µm/km
@Temperature 100 °C
0.70 µm/km
@Temperature 212 °F
 2.2 µm/km
@Temperature 200 °C
2.2 µm/km
@Temperature 392 °F
 2.9 µm/km
@Temperature 240 °C
2.9 µm/km
@Temperature 464 °F
Charpy Impact Unnotched 5.90 J/cm²28.1 ft-lb/in²EN ISO 179/1eU
Charpy Impact, Notched 1.56 J/cm²7.42 ft-lb/in²EN ISO 179/1eA
Coefficient of Friction, Dynamic  0.11
@Temperature 100 °C
0.11
@Temperature 212 °F
Dry Operation
 0.16
@Temperature 20.0 °C
0.16
@Temperature 68.0 °F
Dry Operation
Coefficient of Friction, Static 0.19
@Temperature 20.0 °C
0.19
@Temperature 68.0 °F
Dry Operation
Tensile Creep Modulus, 1000 hours 4320 MPa627000 psiAt 1% Deformation; DIN 53444
Limiting Pressure Velocity 0.54883 MPa-m/sec15669 psi-ft/minv = 1m/min
 0.88333 MPa-m/sec25219 psi-ft/minv = 100m/min
 0.933 MPa-m/sec26600 psi-ft/minv = 200m/min
 1.415 MPa-m/sec40400 psi-ft/minv = 10m/min
Compression Set 4.4 %4.4 %Elastic Compression Limit
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 5.00e+6 ohm-cm5.00e+6 ohm-cmIEC 93
Surface Resistance 3.00e+6 ohm3.00e+6 ohmIEC 93
Dielectric Constant 3.4
@Frequency 110 Hz
3.4
@Frequency 110 Hz
IEC 250
Dissipation Factor 0.000900.00090IEC 112
 0.080
@Frequency 110 Hz
0.080
@Frequency 110 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear  27.0 µm/m-°C
@Temperature <=100 °C
15.0 µin/in-°F
@Temperature <=212 °F
ISO E 830
 29.0 µm/m-°C
@Temperature <=150 °C
16.1 µin/in-°F
@Temperature <=302 °F
ISO E 831
Specific Heat Capacity 1.06 J/g-°C0.253 BTU/lb-°FDSC
Melting Point 390 °C734 °FDSC
Maximum Service Temperature, Air 250 °C482 °FPressed Bushings
 280 °C536 °FContinuous
 320 °C608 °FShort Term (3h)
Deflection Temperature at 1.8 MPa (264 psi) 290 °C554 °FDIN EN ISO 75
Glass Transition Temp, Tg 240 °C464 °FDSC
Flammability, UL94 V-0V-0
 
Descriptive Properties
Alignment Adjustment3Nominal Scale: 1, low; 10, high
Chemical Sterilization10Nominal Scale: 1, low; 10, high
ColorGreen
Creep Resistance6Nominal Scale: 1, low; 10, high
Dimensional Stability with Thermal Expansion10Nominal Scale: 1, low; 10, high
Free from SiliconApplicable
Gamma-rays Radiation Sterilization7Nominal Scale: 1, low; 10, high
Injection Molded PartsApplicable
Machined PartsApplicable
Moist Heat Sterilization6Nominal Scale: 1, low; 10, high
Plastic GranulesApplicable
Resistance Against dust, Dirt, Abrasive Substances5Nominal Scale: 1, low; 10, high
Resistance Against Hot Water120
Resistance to Chemicals5Nominal Scale: 1, low; 10, high
Resistant Against DisinfectantApplicable
Rods up to Øe (de)Applicable
ROHS/WEEEApplicable
Sheets up to Maximum ThicknessApplicable
Sliding Velocity350
Suitable for Outdoor Use9Nominal Scale: 1, low; 10, high
Suitable for VacuumApplicable
Tubes (hollow rods) up to Øe (de)Applicable
UV Rays Resistance9Nominal Scale: 1, low; 10, high

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Wolf Kunststoff ZEDEX® ZX-410V7T A4T Polymer Alloy, Fiber Reinforced, Friction Modified
Plaslok 7021 Black Impact Grade Phenolic Molding Compound
Overview of materials for Epoxy Encapsulant, Unreinforced
Overview of materials for Epoxy, Electrically Conductive
Overview of materials for Silicone, Molded, Glass Fiber Filled

PZEDEX19 / 122134

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.