System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
SABIC XYLEX™ X7300 PC+Polyester (Americas)
Categories:
Polymer
;
Thermoplastic
;
Polycarbonate (PC)
;
Polycarbonate/PET Polyester Blend
Material Notes:
PC+POLYESTER unreinforced alloy. High flow, chemically resistant with excellent optical quality. UV-stabilized.
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.20
g/cc
1.20
g/cc
ASTM D792
Density
1.18
g/cc
0.0426
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.0040
-
0.0080
cm/cm
@Thickness 3.20 mm
0.0040
-
0.0080
in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse
0.0050
-
0.0070
cm/cm
@Thickness 3.20 mm
0.0050
-
0.0070
in/in
@Thickness 0.126 in
SABIC method
Melt Flow
21
g/10 min
@Load 2.16 kg,
Temperature 265 °C
21
g/10 min
@Load 4.76 lb,
Temperature 509 °F
ASTM D1238
21
g/10 min
@Load 2.16 kg,
Temperature 265 °C
21
g/10 min
@Load 4.76 lb,
Temperature 509 °F
cm³/10 min; ISO 1133
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
52.0
MPa
7540
psi
50 mm/min; ASTM D638
55.0
MPa
7980
psi
50 mm/min; ISO 527
Tensile Strength, Yield
49.0
MPa
7110
psi
50 mm/min; ASTM D638
55.0
MPa
7980
psi
50 mm/min; ISO 527
Elongation at Break
150 %
150 %
50 mm/min; ASTM D638
>= 150 %
>= 150 %
50mm/min; ISO 527
Elongation at Yield
5.0 %
5.0 %
50 mm/min; ISO 527
5.0 %
5.0 %
50 mm/min; ASTM D638
Tensile Modulus
1.84
GPa
267
ksi
50 mm/min; ASTM D638
1.90
GPa
276
ksi
1mm/min; ISO 527
Flexural Strength
71.0
MPa
10300
psi
2 mm/min; break; ISO 178
Flexural Yield Strength
83.0
MPa
12000
psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus
1.94
GPa
281
ksi
1.3 mm/min, 50 mm span; ASTM D790
2.00
GPa
290
ksi
2 mm/min; ISO 178
Izod Impact, Notched
6.60
J/cm
12.4
ft-lb/in
ASTM D256
Izod Impact, Notched (ISO)
9.00
kJ/m²
4.28
ft-lb/in²
80*10*4; ISO 180/1A
Dart Drop, Total Energy
95.0
J
70.1
ft-lb
ASTM D3763
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
85.0
µm/m-°C
@Temperature 23.0 - 60.0 °C
47.2
µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
115
µm/m-°C
@Temperature -40.0 - 40.0 °C
63.9
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow
85.0
µm/m-°C
@Temperature 23.0 - 60.0 °C
47.2
µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
105
µm/m-°C
@Temperature -40.0 - 40.0 °C
58.3
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi)
102
°C
@Thickness 3.20 mm
216
°F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
90.0
°C
194
°F
1.8 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
88.0
°C
@Thickness 3.20 mm
190
°F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point
106
°C
223
°F
Rate B/120; ISO 306
108
°C
226
°F
Rate B/50; ASTM D1525
Optical Properties
Metric
English
Comments
Haze
2.0 %
@Thickness 2.54 mm
2.0 %
@Thickness 0.100 in
ASTM D1003
Transmission, Visible
88 %
@Thickness 2.54 mm
88 %
@Thickness 0.100 in
ASTM D1003
Processing Properties
Metric
English
Comments
Nozzle Temperature
250
-
270
°C
482
-
518
°F
Injection Molding
Zone 1
240
-
250
°C
464
-
482
°F
Zone 2
245
-
265
°C
473
-
509
°F
Zone 3
250
-
270
°C
482
-
518
°F
Melt Temperature
250
-
270
°C
482
-
518
°F
Mold Temperature
45.0
-
60.0
°C
113
-
140
°F
Drying Temperature
80.0
-
95.0
°C
176
-
203
°F
Injection Molding
Dry Time
3.00
-
5.00
hour
3.00
-
5.00
hour
Injection Molding
8.00
hour
8.00
hour
Cumulative; Injection Molding
Moisture Content
0.020 %
0.020 %
Back Pressure
0.200
-
0.500
MPa
29.0
-
72.5
psi
Shot Size
40 - 80 %
40 - 80 %
Vent Depth
0.00130
-
0.00200
cm
0.000512
-
0.000787
in
Screw Speed
20
-
100
rpm
20
-
100
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABI11626 / 245093
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.