MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Evonik VESTAMID® DX9303 BK E70288 Nylon 612, Impact Modified, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 612 (PA612); Nylon 612, Impact Modified

Material Notes: VESTAMID® DX9303 BK E70288 is a PA 612 extrusion compound developed for the production of tubing systems with higher requirements for heat resistance. The melting point of VESTAMID® DX9303 BK E70288 is about 35°C higher than PA 11 and PA 12 compounds, allows higher peak temperatures in use. Thereby this compound fulfills the increased demands resulting from higher temperatures in the engine compartment. If it is intended to use VESTAMID® DX9303 BK E70288 for fuel lines, certain preconditions must be observed. The Technical Marketing assists you in finding the suitable VESTAMID® compound. At temperatures above 100°C tubing of VESTAMID® DX9303 BK E70288 allow a higher pressure load than tubing made of PA 12 compounds with comparable flexibility. The process temperatures should be in the range of 240-270°C. The material absorbs only little moisture. Therefore dimensions and properties of parts are nearly unaffected through ambient conditions. Pigmentation may affect values. Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.
Industrial Sector: Automotive and Mobility
Processing: Extrusion
Delivery form: Pellets, Granules
Resistance to: Heat (thermal stability), UV / light / weathering, Oil / fuels
Electrical: Insulating
Conformity: Automotive
Additives: Unfilled
Applications: Tube and hose
Processing: Pipe/Tube extrusion
Special Characteristics: High impact strength, Light-stabilized, High heat resistant , High viscosity
Color: Black
Additives: Impact resistant, Light stabilizer, Heat stabilizer

Information provided by Evonik.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 65.0
@Time 3.00 sec
ISO 7619-1
Tensile Strength at Break 41.0 MPaISO 527
Elongation at Break >= 200 %nom. strain at br., etB; ISO 527
 200 %Nominal; ISO 527
Tensile Modulus 680 MPaISO 527
Flexural Strength 18.0 MPaat conv. Deflection; ISO 178
 28.0 MPaISO 178
Flexural Modulus 605 MPaISO 178
Flexural Strain at Break 10.0 %at flexural strength; ISO 178
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179/1eU
 NB
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 15.0 kJ/m²
@Temperature -30.0 °C
Type of failure: C(P); ISO 179/1eA
 135 kJ/m²
@Temperature 23.0 °C
Type of failure: P; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 5.30e+8 ohm-cm?V; IEC 62631-3-1
Surface Resistance 5.00e+12 ohmsC, circular electrodes; IEC 62631-3-2
Dielectric Strength 34.0 kV/mmAC, S20/S20, t.; IEC 60243-1
 
Processing PropertiesOriginal ValueComments
Melt Temperature 250 °CInjection Molding; ISO 294
Mold Temperature 80.0 °CInjection Molding; ISO 294
Injection Velocity 200 mm/secInjection Molding; ISO 294
 
Descriptive Properties
Blue water consumption22.2 kgISO 14040, 14044
ColorBlack
Flexural stress at breakNMPa, ISO 178
 N%, ISO 178
Global Warming Potential2.4 kg CO2 eq./kgsavings incl. bio. C. as compared to classical production, ISO 14040, 14044
 6.9 kg CO2 eq./kgincl. bio. C incl. LUC, ISO 14040, 14044
 6.9 kg CO2 eq./kgexcl. bio. C incl. LUC, ISO 14040, 14044
Land use (ReCiPe 2016)0.3 Annual crop eq. yISO 14040, 14044

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEVONIK7887 / 325019

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.