System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
LG Chemical LUPOY SR3108FM PC, Halogen Free Flame Retardance
Categories:
Polymer
;
Thermoplastic
;
Polycarbonate (PC)
;
Polycarbonate, Unreinforced, Flame Retardant
Material Notes:
Description: Injection Molding, PC, Halogen Free Flame Retardance, Light Reflectance, White Color Only
Application: LCD Back Light Unit parts
CAS: 103598-77-2, 9003-56-9 and 13463-67-1
Information provided by LG Chemical
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.25
g/cc
1.25
g/cc
ASTM D792
Maximum Moisture Content
0.020
0.020
Injection Molding
Linear Mold Shrinkage, Flow
0.0050
-
0.0080
cm/cm
@Thickness 3.20 mm
0.0050
-
0.0080
in/in
@Thickness 0.126 in
ASTM D955
Melt Flow
15
g/10 min
@Load 1.20 kg,
Temperature 300 °C
15
g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
117
117
ASTM D785
Tensile Strength, Yield
57.9
MPa
@Thickness 3.20 mm
8390
psi
@Thickness 0.126 in
50mm/min; ASTM D638
Elongation at Break
120 %
@Thickness 3.20 mm
120 %
@Thickness 0.126 in
50mm/min; ASTM D638
Flexural Yield Strength
93.2
MPa
@Thickness 3.20 mm
13500
psi
@Thickness 0.126 in
10mm/min; ASTM D790
Flexural Modulus
2.45
GPa
@Thickness 3.20 mm
356
ksi
@Thickness 0.126 in
10mm/min; ASTM D790
Izod Impact, Notched
>=
6.37
J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
>=
11.9
ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
Electrical Properties
Metric
English
Comments
Arc Resistance
0.00
-
60
sec
0.00
-
60
sec
ASTM D495
Comparative Tracking Index
400
-
600
V
400
-
600
V
Hot Wire Ignition, HWI
15
-
30
sec
@Thickness >=1.50 mm
15
-
30
sec
@Thickness >=0.0591 in
30
-
60
sec
@Thickness >=3.00 mm
30
-
60
sec
@Thickness >=0.118 in
High Amp Arc Ignition, HAI
>=
120
arcs
@Thickness 1.50 mm
>=
120
arcs
@Thickness 0.0591 in
>=
120
arcs
@Thickness 3.00 mm
>=
120
arcs
@Thickness 0.118 in
High Voltage Arc-Tracking Rate, HVTR
80.0
-
150
mm/min
3.15
-
5.91
in/min
Thermal Properties
Metric
English
Comments
Deflection Temperature at 1.8 MPa (264 psi)
>=
127
°C
@Thickness 6.40 mm
>=
261
°F
@Thickness 0.252 in
Unannealed; ASTM D648
UL RTI, Electrical
80.0
°C
@Thickness >=0.850 mm
176
°F
@Thickness >=0.0335 in
110
°C
@Thickness >=1.50 mm
230
°F
@Thickness >=0.0591 in
110
°C
@Thickness >=3.00 mm
230
°F
@Thickness >=0.118 in
UL RTI, Mechanical with Impact
80.0
°C
@Thickness >=0.850 mm
176
°F
@Thickness >=0.0335 in
100
°C
@Thickness >=1.50 mm
212
°F
@Thickness >=0.0591 in
100
°C
@Thickness >=3.00 mm
212
°F
@Thickness >=0.118 in
UL RTI, Mechanical without Impact
80.0
°C
@Thickness >=0.850 mm
176
°F
@Thickness >=0.0335 in
120
°C
@Thickness >=1.50 mm
248
°F
@Thickness >=0.0591 in
120
°C
@Thickness >=3.00 mm
248
°F
@Thickness >=0.118 in
Flammability, UL94
V-1
@Thickness >=0.850 mm
V-1
@Thickness >=0.0335 in
V-0
@Thickness >=1.50 mm
V-0
@Thickness >=0.0591 in
V-0
@Thickness >=3.00 mm
V-0
@Thickness >=0.118 in
Processing Properties
Metric
English
Comments
Rear Barrel Temperature
250
-
280
°C
482
-
536
°F
Injection Molding
Middle Barrel Temperature
260
-
290
°C
500
-
554
°F
Injection Molding
Front Barrel Temperature
260
-
290
°C
500
-
554
°F
Injection Molding
Nozzle Temperature
260
-
280
°C
500
-
536
°F
Injection Molding
Melt Temperature
260
-
280
°C
500
-
536
°F
Injection Molding
Mold Temperature
60.0
-
90.0
°C
140
-
194
°F
Injection Molding
Drying Temperature
100
-
120
°C
212
-
248
°F
Injection Molding
Dry Time
4.00
-
6.00
hour
4.00
-
6.00
hour
Injection Molding
Back Pressure
0.981
-
3.92
MPa
142
-
569
psi
Injection Molding
Screw Speed
40
-
70
rpm
40
-
70
rpm
Injection Molding
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
LG Chemical LUPOY SR3108FC PC, Halogen Free Flame Retardance
Lotte Advanced Materials Infino® HN-1064IA PC, Unreinforced FR
Westlake Plastics Radel® R 5500 Polyphenylsulfone
PTS Tristar® PC-10FR-(VIM) 12 MFI Flame Retardant, UV Stabilized Polycarbonate With Release
Polymer Resources PC-FR2-D-[color]-3 Polycarbonate, Improved Flame Retardant, Medium Flow, UV-stabilized
PLAY561 / 148571
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.