MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow Elvax® 3135X Ethylene-Vinyl Acetate Copolymer Resin for Thin Blown
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: 12 wt% Vinyl Acetate.

Elvax® 3135X is an extrudable, ethylene-vinyl acetate copolymer resin available in pellet form for use in conventional extrusion equipment designed to process polyethylene resins.

Applications: Elvax® 3135X is designed to provide a low-temperature heat seal to itself or many other materials commonly used in flexible packaging applications. The melt properties of this resin allow it to be processed on blown film equipment over a wide range of film thicknesses and blow-up ratios. It can also be coextruded with a variety of other polymers. Films from this resin exhibit good puncture resistance, superior optics, a high degree of stretch, and are often used in stretch wrap and/or stretch bundling applications. Elvax® 3135X is also available in a specially formulated compound (Elvax® 3135AC) for those applications requiring added cling.

Information provided by DuPont Packaging Polymers.

This former DuPont product line is now a Dow product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.930 g/ccASTM D792
Moisture Vapor Transmission 0.910 cc-mm/m²-24hr-atm
@Thickness 0.0254 mm
g-mm/m²-day; based on film thickness; ASTM E96; ASTM E96
Oxygen Transmission 201 cc-mm/m²-24hr-atm
@Thickness 0.0254 mm
film; ASTM D3985
Viscosity 2.00e+6 cP
@Shear Rate 50 1/s,
Temperature 190 °C
estimated from log-log graph
Melt Flow 0.35 g/10 minCondition not noted.; ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 550 %50 µm (2 mil) film; ASTM D882
Film Elongation at Break, TD 550 %50 µm (2 mil) film; ASTM D882
Secant Modulus, MD 0.0580 GPa50 µm (2 mil) film; ASTM D882
Secant Modulus, TD 0.0650 GPa50 µm (2 mil) film; ASTM D882
Impact 43.6J/mm Spencer Impact; Average of MD and TD; ASTM D3420
Coefficient of Friction 1.3film/metal; ASTM D1894
 3.4film/film; ASTM D1894
Elmendorf Tear Strength, MD 81.0 g/mil50 µm (2 mil) film; ASTM D1922
Elmendorf Tear Strength, TD 85.0 g/mil50 µm (2 mil) film; ASTM D1922
Film Tensile Strength at Break, MD 32.0 MPa50 µm (2 mil) film; ASTM D882
Film Tensile Strength at Break, TD 34.0 MPa50 µm (2 mil) film; ASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 78.0 °CFreezing Point via DSC/ASTM D3418
 95.0 °CUpon Melting via DSC/ASTM D3418
Vicat Softening Point 82.0 °CASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 3.0 %ASTM D1003
Gloss 123 %20°; ASTM D2457
Transmission, Visible 69 %50 µm (2 mil) film; ASTM D1746
 
Processing PropertiesOriginal ValueComments
Melt Temperature 175 - 205 °Cblown film extrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow Elvax® 3120 Ethylene-Vinyl Acetate Copolymer Resin for Blown Film
Dow Elvax® 3130 Ethylene-Vinyl Acetate Copolymer Resin for Blown Film
Dow Elvax® 3135SB Ethylene-Vinyl Acetate Copolymer Resin for Blown Film
Dow Elvax® 3150 Ethylene-Vinyl Acetate Copolymer Resin for Coextrusion, Blown Film
Dow Elvax® 760 Ethylene Vinyl Acetate

PDUPH9 / 33612

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.