MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Copper nickel 30%, UNS C71500, OSO25 Temper 25 mm tubing
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Excellent corrosion resistance. Good hot and cold workability. Fabricated by forming and bending, welding.

Applications: condensers, condenser plates, distiller tubing, evaporator and heat exchanger tubing, ferrules, salt water piping.

Test specimen: tubing - 25mm OD x 1.65mm wall thickness.

Key Words: CDA 715 (70/30); 70-30 Cupronickel
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.94 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 45
Tensile Strength, Ultimate 415 MPa
Tensile Strength, Yield 170 MPa
@Strain 0.5 %
Elongation at Break 45 %In 50 mm
Modulus of Elasticity 150 GPa
Poissons Ratio 0.32Calculated
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 57.0 GPa
Charpy Impact 107 JKeyhole; temper not reported
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000375 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.380 J/g-°C
Thermal Conductivity 29.0 W/m-K
@Temperature 20.0 °C
 29.2 W/m-K
@Temperature 100 °C
Mill Annealed
 34.1 W/m-K
@Temperature 200 °C
Mill Annealed
 38.6 W/m-K
@Temperature 300 °C
Mill Annealed
 43.1 W/m-K
@Temperature 400 °C
Mill Annealed
 48.1 W/m-K
@Temperature 500 °C
Mill Annealed
 53.1 W/m-K
@Temperature 600.0 °C
Mill Annealed
 58.1 W/m-K
@Temperature 700.0 °C
Mill Annealed
Melting Point 1170 - 1240 °C
Solidus 1170 °C
Liquidus 1240 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 650 - 825 °C
Hot-Working Temperature 925 - 1050 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 70 %
Iron, Fe 0.40 - 0.70 %
Lead, Pb <= 0.050 %
Manganese, Mn <= 1.0 %
Nickel, Ni 29 - 33 %
Other, total <= 0.50 %
Zinc, Zn <= 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Copper nickel 30%, UNS C71500
Copper nickel 30%, UNS C71500, O61 Temper 19 mm tubing
Copper nickel 30%, UNS C71500, H80 Temper 1 mm strip
Copper nickel 30%, UNS C71500, O61 Temper 1 mm strip
Copper nickel 30%, UNS C71500, H02 Temper 25 mm rod

MC71500b6 / 11749

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.