MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI 4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs., tested at -195°C (-320°F)  (Unverified Data**)
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: AISI 4340 has a favorable response to heat treatment (usually oil quenching followed by tempering) and exhibits a good combination of ductility and strength when treated thusly. Uses include piston pins, bearings, ordnance, gears, dies, and pressure vessels.

Key Words: alloy steels, UNS G43400, AMS 5331, AMS 6359, AMS 6414, AMS 6415, ASTM A322, ASTM A331, ASTM A505, ASTM A519, ASTM A547, ASTM A646, MIL SPEC MIL-S-16974, SAE J404, SAE J412, SAE J770, DIN 1.6565, JIS SNCM 8, IS 1570 40Ni2Cr1Mo28, IS 1570 40NiCr1Mo15
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 666666Converted from Vickers hardness.
Hardness, Vickers 639639
Tensile Strength, Ultimate 2200 MPa319000 psi
Tensile Strength, Yield 1915 MPa277700 psi
Elongation at Break 10 %10 %
Reduction of Area 24 %24 %
Modulus of Elasticity 211 GPa30600 ksi
Bulk Modulus 160 GPa23200 ksiTypical for steel.
Poissons Ratio 0.300.30Calculated
Machinability 50 %50 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 81.0 GPa11700 ksiEstimated from elastic modulus
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000248 ohm-cm
@Temperature 20.0 °C
0.0000248 ohm-cm
@Temperature 68.0 °F
 0.0000298 ohm-cm
@Temperature 100 °C
0.0000298 ohm-cm
@Temperature 212 °F
 0.0000552 ohm-cm
@Temperature 400 °C
0.0000552 ohm-cm
@Temperature 752 °F
 0.0000797 ohm-cm
@Temperature 600 °C
0.0000797 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.4 µm/m-°C
@Temperature 20.0 °C
5.78 µin/in-°F
@Temperature 68.0 °F
specimen oil hardened, 630°C (1110°F) temper
 12.6 µm/m-°C
@Temperature 21.0 - 260 °C
7.00 µin/in-°F
@Temperature 69.8 - 500 °F
1.88% Ni, normalized and tempered
 13.7 µm/m-°C
@Temperature 21.0 - 540 °C
7.61 µin/in-°F
@Temperature 69.8 - 1000 °F
1.88% Ni, normalized and tempered
 13.9 µm/m-°C
@Temperature 21.0 - 540 °C
7.72 µin/in-°F
@Temperature 69.8 - 1000 °F
1.90% Ni, quenched, tempered
Specific Heat Capacity 0.475 J/g-°C0.114 BTU/lb-°FTypical 4000 series steel
Thermal Conductivity 44.5 W/m-K309 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.37 - 0.43 %0.37 - 0.43 %
Chromium, Cr 0.70 - 0.90 %0.70 - 0.90 %
Iron, Fe 95.195 - 96.33 %95.195 - 96.33 %As remainder
Manganese, Mn 0.60 - 0.80 %0.60 - 0.80 %
Molybdenum, Mo 0.20 - 0.30 %0.20 - 0.30 %
Nickel, Ni 1.65 - 2.0 %1.65 - 2.0 %
Phosphorus, P <= 0.035 %<= 0.035 %
Silicon, Si 0.15 - 0.30 %0.15 - 0.30 %
Sulfur, S <= 0.040 %<= 0.040 %

References for this datasheet.

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs.
AISI 4340 Steel, oil quenched 845°C, 425°C (800°F) temper
AISI 4340 Steel, oil quenched 800°C (1470°F), 540°C (1000°F) temper, 13 mm (0.5 in.) round
AISI 4340 Steel, annealed, 25 mm round
AISI 4340 Steel, oil quenched 800°C (1470°F), 540°C (1000°F) temper, 100 mm (4 in.) round

M434AX / 7774

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.