MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Westlake LF 2032 LLDPE  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Injection Molded

Material Notes: Applications
  • Bags and Sacks
  • Agricultural Films
  • Trash Bags and Liners
  • Coextruded Structures
Properties
  • Excellent Stiffness
  • Excellent Tear Strength

FDA: This material complies with FDA regulations in 21 CFR, section 177.1520, paragraph C, section 3.1a. Kosher approved

Processing: Melt temperatures of 400° to 440°F are recommended for Westlake Polymers LF 2032 with blow-up ratios of 2:1 or higher.

Information provided by Westlake Chemical Corporation

Key Words: Agricultural Films, Trash Bags and Liners, Coextruded Structures
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.917 g/ccASTM D1505
Thickness 1.00 milWESTLAKE
Melt Flow 0.80 g/10 minASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 1400 psiASTM D882
Film Tensile Strength at Yield, TD 1500 psiASTM D882
Film Elongation at Break, MD 650 %ASTM D882
Film Elongation at Break, TD 900 %ASTM D882
Elmendorf Tear Strength MD 350 gASTM D1922A
Elmendorf Tear Strength TD 650 gASTM D1922A
Dart Drop 500 g/milCalculated
Dart Drop Test 500 gASTM D1709A
Film Tensile Strength at Break, MD 6200 psiASTM D882
Film Tensile Strength at Break, TD 4500 psiASTM D882
1% Secant Modulus, MD 26000 psiASTM D882
1% Secant Modulus, TD 32000 psiASTM D882
 
Optical PropertiesOriginal ValueComments
Haze 11 %Unformulated polymer only; ASTM D1003
 
Processing PropertiesOriginal ValueComments
Melt Temperature 400 - 440 °F
 
Compliance PropertiesOriginal ValueComments
FDA Yes
 
Descriptive Properties
ProcessFilm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chevron Phillips Marlex® 9006 HDPE Injection Molding Resin
PolyMirae Moplen EP500N Injection Molding Grade Polypropylene
Westlake Hifor LT74107-F Polyethylene Film, Using Energx Technology Services
Westlake EC477AA Low Density Polyethylene
Westlake EC476AA Low Density Polyethylene

PWESG041 / 72687

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.