MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Low-leaded brass tube, UNS C33000
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Fair to excellent corrosion resistance. Combines good machinability and excellent cold workability. Fabricated by forming and bending, machining, piercing and punching.

Applications: pump and power cylinders and liners, ammunition primers, plumbing accessories.

Available as tube.

Key Words: CDA 330
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.50 g/cc0.307 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 324 - 517 MPa47000 - 75000 psi
Tensile Strength, Yield 103 - 414 MPa14900 - 60000 psiDepending on temper
Elongation at Break 60 %60 %in 177.8 mm.
Modulus of Elasticity 105 GPa15200 ksi
Poissons Ratio 0.350.35Calculated
Machinability 60 %60 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 39.0 GPa5660 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000660 ohm-cm0.00000660 ohm-cm26% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.2 µm/m-°C
@Temperature 20.0 - 300 °C
11.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 115 W/m-K
@Temperature 20.0 °C
798 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 905 - 940 °C1660 - 1720 °F
Solidus 905 °C1660 °F
Liquidus 940 °C1720 °F
Annealing Point 427 - 649 °C800 - 1200 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 65 - 68 %65 - 68 %
Iron, Fe <= 0.070 %<= 0.070 %
Lead, Pb 0.20 - 0.80 %0.20 - 0.80 %
Other, total <= 0.50 %<= 0.50 %
Zinc, Zn 33.5 %33.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Low-leaded brass, UNS C33500
Free-Cutting Brass, UNS C36000
Forging Brass, UNS C37700
High-leaded brass, 62%, UNS C35300
High-leaded brass, UNS C34200

MC33000b1 / 11167

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.