MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
RTP Company RTP 2187 L  Polyetherimide (PEI) Carbon Fiber 40% - Lubricated  (discontinued **)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI); Polyetherimide (PEI), Carbon Fiber Filled

Material Notes: Carbon Fiber 40% - Lubricated

Comments:

  • Carbon Fiber
  • Lubricated

Unless otherwise specified, all data listed is for natural or black colored materials. Pigments can affect properties.

Information provided by RTP Company.


Data for this product has not been recently verified, please contact RTP Company for more information before specifying this grade.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.44 g/ccASTM D792
Filler Content 40 %
Water Absorption 0.18 %24 hours at 23°C; ASTM D570
Linear Mold Shrinkage 0.00050 cm/cm
@Thickness 3.17 mm
ASTM D955
 0.0010 cm/cm
@Thickness 6.35 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 34000 psiASTM D638
Elongation at Break 1.0 %ASTM D638
Modulus of Elasticity 4500 ksiASTM D638
Flexural Yield Strength 48000 psiASTM D790
Flexural Modulus 3200 ksiASTM D790
Izod Impact, Notched 1.30 ft-lb/in
@Thickness 3.17 mm
ASTM D256
Izod Impact, Unnotched 21.0 ft-lb/in
@Thickness 3.17 mm
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1e+05ASTM D257
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 415 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 410 °FASTM D648
 
Processing PropertiesOriginal ValueComments
Processing Temperature 660 - 720 °F
Mold Temperature 275 - 350 °F
Injection Pressure 12000 - 18000 psi
 
Descriptive Properties
ColorNatural/Black

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LNP ULTEM® SMU5836 Polyetherimide, 30% Carbon Fiber Reinforcement
PlastiComp Complet® LCF40-PEI Polyetherimide, 40% Long Carbon Fiber Reinforced
LNP ULTEM® UC3000 Polyetherimide, 30% Carbon Fiber Reinforcement
Akro-Plastic Akrotek® PEEK CF 40 9 black (5182) PEEK, Dry, 40% Carbon Filled

PR4944 / 64279

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.