MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 1060 Steel, oil quenched 845°C (1550°F), 480°C (900°F) temper, 100 mm (4 in.) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; High Carbon Steel

Material Notes: Applications include battering tools, hot upset forging dies, ring-rolling tools, wear-resistant parts, hand tools, and parts for agricultural implements. Post oil quenched hardness: 29 HRC surface, 26 HRC half-radius, 24 HRC center.

Key Words: UNS G10600, AMS 7240, ASTM A29, ASTM A510, ASTM A576, ASTM A682, carbon steels, MIL SPEC MIL-S-16974, SAE J403, SAE J412, SAE J414, DIN 1.0601, AFNOR CC 55 (Fr), UNI C 60, B.S. 060 A 62
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.87 g/ccTypical for steel.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 269
Hardness, Knoop 294Converted from Brinell
Hardness, Rockwell B 99Converted from Brinell
Hardness, Rockwell C 27Converted from Brinell
Hardness, Vickers 284Converted from Brinell
Tensile Strength, Ultimate 931 MPa
Tensile Strength, Yield 518 MPa
Elongation at Break 18.2 %in 50 mm
Reduction of Area 44.8 %
Modulus of Elasticity 200 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel.
Poissons Ratio 0.29Typical For Steel
Shear Modulus 80.0 GPaTypical for steel.
Izod Impact 11.0 Jannealed at 790°C (1450°F)
 14.0 Jnormalized at 900°C (1650°F)
 18.0 Jas rolled
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000180 ohm-cm
@Temperature 20.0 °C
condition of specimen unknown
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.0 µm/m-°C
@Temperature 20.0 - 100 °C
 11.5 µm/m-°C
@Temperature 20.0 - 200 °C
 12.2 µm/m-°C
@Temperature 20.0 - 300 °C
 13.1 µm/m-°C
@Temperature 20.0 - 400 °C
 13.7 µm/m-°C
@Temperature 20.0 - 500 °C
 14.0 µm/m-°C
@Temperature 20.0 - 600 °C
 14.4 µm/m-°C
@Temperature 20.0 - 700 °C
Specific Heat Capacity 0.502 J/g-°C
@Temperature >=100 °C
condition unknown
 0.544 J/g-°C
@Temperature 150 - 200 °C
Thermal Conductivity 51.9 W/m-KTypical steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.55 - 0.66 %
Iron, Fe 98.35 - 98.85 %As remainder
Manganese, Mn 0.60 - 0.90 %
Phosphorus, P <= 0.040 %
Sulfur, S <= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1060 Steel, normalized at 900°C (1650°F), air cooled, 100 mm (4 in.) round
AISI 1080 Steel, oil quenched from 815°C (1500°F), 480°C (900°F) temper, 100 mm (4 in.) round
AISI 1060 Steel, cold drawn, spheroidized annealed, 19-32 mm (0.75-1.25 in) round
AISI 1060 Steel, oil quenched 845°C (1550°F), 540°C (1000°F) temper, 100 mm (4 in.) round
AISI 1064 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round

M1060N / 7060

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.