MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
African Mahogany Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Excellent shaping, very good planing, fair steam bending. Data is based on small, clear, air-dried samples unless specified.
Usual surface texture: Medium
Dimensional changes when dried lumber is subjected to variations in humidity during service: Small
Resistance to fungal decay (Heartwood in ground contact): Moderately Durable (10 to 15 years)
Resistance to penetration by preservatives: Extremely resistant
Common Applications: Furniture, cabinet work, boat building, joinery

Key Words: Khaya ivorensis; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.420 g/ccGreen
Density 0.510 g/ccAir Dry (12-15% Moisture Content)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Wood Indentation 2800 NSide Hardness, Green
 3700 NSide Hardness, 12% Moisture
Tensile Strength, Ultimate 2.00 MPaPerpendicular to Grain
 60.0 MPaAxial
Modulus of Rupture 0.0510 GPaStatic Bending, Green
 0.0738 GPaStatic Bending, 12% Moisture
 0.0740 GPaIn Bending
Flexural Modulus 9.80 - 10.2 GPaIn Bending
 7900 MPaStatic Bending, Green
 9700 MPaStatic Bending, 12% Moisture
Compressive Strength 6.90 MPaPerpendicular to Grain
 25.7 MPaParallel to Grain, Green
 39.3 - 45.0 MPaParallel to Grain
 44.5 MPaParallel to Grain, 12% Moisture
Poissons Ratio 0.032µTL, 12% Moisture Content
 0.033µRL, 12% Moisture Content
 0.264µTR, 12% Moisture Content
 0.297µLR, 12% Moisture Content
 0.604µRT, 12% Moisture Content
 0.641µLT, 12% Moisture Content
Machinability 50 %Medium Relative to Other Wood
Shear Strength 6.40 MPaParallel to Grain, Green
 7.80 MPaOrientation Unknown
 10.3 MPaParallel to Grain, 12% Moisture
Impact 3.9J/cm² Toughness
Work to Maximum Load 0.0490 J/cm³Static Bending, Green
 0.0570 J/cm³Static Bending, 12% Moisture
 
Thermal PropertiesOriginal ValueComments
Shrinkage 2.5 %Radial Shrinkage Green to Oven Dry
 4.5 %Tangential Shrinkage Green to Oven Dry
 8.8 %Volumetric Shrinkage Green to Oven Dry
 
Descriptive Properties
ColorReddish-brownUsual for heartwood

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Tropical American Mahogany Wood
Teak Wood
American Pine Wood
American Red Oak Wood
American White Ash Wood

PTSIE / 71348

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.