MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Zytel® (PA66) NVH70G35HSLA BK152 PA66-IGF35  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Glass Fiber Filled

Material Notes: 35% Glass Reinforced, Heat Stabilized, Polyamide 66 with improved damping performance

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.42 g/ccDAM; ISO 1183
Water Absorption 1.8 %
@Thickness 1.00 mm,
Time 86400 sec
Sim. to ISO 62
Moisture Absorption 1.20 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.010 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 105 MPa50%RH; ISO 527-1/-2
 145 MPaDAM; ISO 527-1/-2
Elongation at Break 2.5 %DAM; ISO 527-1/-2
 3.5 %50%RH; ISO 527-1/-2
Tensile Modulus 8300 MPa50%RH; ISO 527-1/-2
 10200 MPaDAM; ISO 527-1/-2
Flexural Strength 170 MPa50%RH; ISO 178
 220 MPaDAM; ISO 178
Flexural Modulus 7900 MPa50%RH; ISO 178
 9200 MPaDAM; ISO 178
Poissons Ratio 0.34DAM
 0.3450%RH
Izod Impact, Notched (ISO) 8.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 13.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
Izod Impact, Unnotched (ISO) 62.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1U
 63.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1U
Charpy Impact Unnotched 60.0 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eU
 60.0 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eU
 67.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 70.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 7.00 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eA
 8.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 11.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 11.0 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 248 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 237 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 35.0 °C10°C/min; 50%RH; ISO 11357-1/-2
 75.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
DAM; IEC 60695-11-10
 
Processing PropertiesOriginal ValueComments
Melt Temperature 275 - 295 °CInjection
 285 °COptimum, Injection
Mold Temperature 50.0 - 100 °CInjection
 90.0 °COptimum, Injection
Drying Temperature 80.0 °C
@Time 7200 - 14400 sec
Injection; Dehumidified Dryer
Moisture Content 0.20 %
Hold Pressure 50.0 - 100 MPaInjection
 
Descriptive Properties
AdditivesLubricants
 Release agent
Delivery formPellets
Drying Recommendedyes
FeaturesHeat stabilized or stable to heat
Hold pressure time (s/mm)3Injection
ISO designationISO 16396-PA66-I,GF35,M1CGHR,S14-100
Max. screw tangential speed (m/s)0.2
Part Marking Code>PA66-IGF35<ISO 11469
ProcessingInjection Molding
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPA66-IGF35ISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDSX5481m / 254533

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.