MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Samyang Tribit® 1500N Polybutylene Terephthalate, Flame Retardant  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Flame Retardant

Material Notes: Characteristics:
  • UL 94 V-0

Applications:

  • Automotive
    • Connector
    • Gear
    • Outdoor handle
    • Ignition system
  • Electronic
    • Connector
    • Gas valve
    • Coil bobbin
    • Switch case
    • Relay case
  • O/A parts

All information provided by Samyang

Key Words: PBT
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.42 g/ccASTM D792
Water Absorption 0.080 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage 0.013 - 0.018 cm/cm
@Thickness 3.00 mm
ASTM D955
Melt Flow 60 g/10 min
@Load 2.16 kg,
Temperature 235 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 118ASTM D785
Tensile Strength, Yield 560 kg(f)/cm²ASTM D638
Elongation at Break 40 %ASTM D638
Flexural Yield Strength 850 kg(f)/cm²ASTM D790
Flexural Modulus 25000 kg(f)/cm²ASTM D790
Izod Impact, Unnotched 6.00 kg-cm/cm
@Thickness 3.17 mm
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmASTM D257
Dielectric Constant 3.2
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 18.0 kV/mmASTM D149
Dissipation Factor 0.020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 71 secASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 90.0 µm/m-°CASTM D696
Melting Point 226 °C
Deflection Temperature at 0.46 MPa (66 psi) 150 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 165 °CASTM D648
Flammability, UL94 V-0
@Thickness 1.59 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 230 - 240 °C
Middle Barrel Temperature 220 - 240 °C
Front Barrel Temperature 200 - 220 °C
Nozzle Temperature 230 - 240 °C
Melt Temperature 245 °C
Drying Temperature 110 - 130 °C
Dry Time 4 - 6 hour
Moisture Content 0.010 - 0.015 %
Screw Speed 40 - 60 rpm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Samyang Tribit® 1700S Polybutylene Terephthalate
Samyang Tribit® 1503S Polybutylene Terephthalate
Samyang Tribit® 1501N PBT, Flame Retardancy
Samyang Tribit® 1500 Polybutylene Terephthalate

PSAMY044 / 88126

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.