MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
RESPOL REPSOL PRIMEVA® P2870 EVA
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate; Molded/Extruded

Material Notes: Product Description: EVA copolymer REPSOL PRIMEVA® P2870 is recommended for hot melt adhesives applications, injection molding and extrusion of profiles. It contains antioxidant and free flowing agent.
Applications: Injection molding. Release agents containing silicone must be avoided; Hot Melt Adhesives – Packaging, Edge veneering, Shoe industry; Manufacture of masterbatches; Microcellular foams; Manufacture of sonic damping sheets
Recommended melt temperature below 200°C to avoid the decomposition of the polymer. Processing conditions should be optimized for each production line.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Additive: Antioxidant; Free Flowing Agent

Features: Antioxidant; Copolymer; Food Contact Acceptable

Uses: Adhesives; Foam; Footwear; Masterbatch; Packaging; Sheet

Agency Ratings: EU Food Contact

Processing Method: Injection Molding; Profile Extrusion

Information provided by REPSOL

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.950 g/ccISO 1183
Brookfield Viscosity 1.77e+6 cP
@Temperature 200 °C
Spindle SC4-27
Vinyl Acetate Content 28 %
Melt Flow 7.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 80ISO 868
Hardness, Shore D 28ISO 868
Tensile Strength at Break 3190 psiISO 527-2
Elongation at Break 760 %ISO 527-2
 
Thermal PropertiesOriginal ValueComments
Melting Point 160 °F
Ring & Ball Softening Point 288 °FASTM E28
 
Processing PropertiesOriginal ValueComments
Melt Temperature 392 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PRESPOL1328 / 312021

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.