MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilamid® 1S XE 4224 nat PA1010
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Grilamid XE 4224 natural is a heat and UV stabilized high viscosity polyamide 1010 (PA1010), designed for extrusion. In addition the product can be used for thicker injection molded articles.

Grilamid XE 4224 is characterized by the following product profile:

  • Close to 100% based on renewable resources
  • Good chemical and UV resistance
  • Ductile, resilient
  • Low moisture absorption
  • High dimensional stability
  • Low density
Grilamid XE 4224 natural is suitable for applications in areas like:
  • Consumer goods
  • Automotive functional parts
  • Semi-fabricates
  • Tubes, film, sheet, profiles
  • Cable sheathing and protection

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccDry; ISO 1183
Water Absorption 2.1 %Sim. to ISO 62
Moisture Absorption 1.00 %Sim. to ISO 62
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 80.0 MPaConditioned; ISO 2039-1
 110 MPaDry; ISO 2039-1
Tensile Strength, Yield 50.0 MPaConditioned; ISO 527-1/-2
 55.0 MPaDry; ISO 527-1/-2
Elongation at Break 30 %Nominal, Dry; ISO 527-1/-2
 45 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 5.0 %Dry; ISO 527-1/-2
 20 %Conditioned; ISO 527-1/-2
Tensile Modulus 1300 MPaConditioned; ISO 527-1/-2
 2000 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched NB
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
Dry; ISO 179/1eU
Charpy Impact, Notched 6.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
 6.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 9.00 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+9 ohm-cmDry; IEC 60093
 1.00e+9 ohm-cmConditioned; IEC 60093
Surface Resistance 1.00e+10 ohmIEC 60093
Dielectric Strength 38.0 kV/mmDry; IEC 60243-1
 38.0 kV/mmConditioned; IEC 60243-1
Comparative Tracking Index 600 VConditioned; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 110 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 80.0 µm/m-°CISO 11359-1/-2
Melting Point 200 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 125 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 50.0 °CISO 75-1/-2
Flammability, UL94 HBIEC 60695-11-10
 
Descriptive Properties
AutomotivePowertrain and Chassis
Electricals & ElectronicsCables & Tubes
 Connectors
FormGranules
Industry & Consumer goodsHousewares
 Mechanical Engineering
 Sports & Leisure
 Tools & Accessories
ProcessingFilm Extrusion
 Other Extrusion
Product AttributesBio based Polyamide
 High viscosity
 Nucleated
Special CharacteristicsImproved heat resistance
 Improved UV resistance (outdoor use)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
EMS-Grivory Grilamid® TR 55 LX PA12/MACMI
Avient PolyOne® 1005 White PEC Polyethylene
A. Schulman POLYBATCH™ Bright White LL80250 Concentrate Based In LLDPE
3M Dyneon™ Fluorel™ Dipolymer, 22% Carbon Black Filled
304 Stainless Steel

PGRH001 / 156710

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.